Leather trim panel skin hidden tear seam with disrupted fiber matrix
09771044 ยท 2017-09-26
Assignee
Inventors
- Manoj Kumar Patnala (Canton, MI, US)
- Bari W. Brown (Ann Arbor, MI, US)
- Frank Q. Liu (Canton, MI, US)
- Alan M. Perelli (Plymouth, MI, US)
Cpc classification
International classification
B60R21/2165
PERFORMING OPERATIONS; TRANSPORTING
B60R21/217
PERFORMING OPERATIONS; TRANSPORTING
Abstract
A vehicle interior trim system such as an instrument panel or a door panel includes a panel substrate defining a deployment aperture. An inflatable device such as an air bag is adapted to deploy through the aperture during a crash. A natural, tanned leather skin covers the substrate, wherein the skin has a tear seam corresponding to the aperture on a hidden surface of the skin. An aperture door may be fitted within the deployment aperture which is adapted to open against the skin in response to deployment of the inflatable device. The tear seam is comprised of a region on the hidden surface of the skin having a disrupted fiber matrix from exposure to an alkaline solution such as ammonia, bleach, sodium tetraborate, sodium hydroxide, sodium bicarbonate, trisodium phosphate, potassium hydroxide, and potassium carbonate.
Claims
1. A vehicle system comprising: a substrate forming an interior trim panel and defining a deployment aperture; an inflatable device adapted to deploy through the aperture; and a leather skin covering the substrate, wherein the skin has a tear seam corresponding to the aperture on a hidden surface of the skin, and wherein the tear seam is comprised of a region of the skin having a disrupted fiber matrix from exposure to an alkaline solution.
2. The system of claim 1 wherein a door is fitted within the deployment aperture adapted to open against the skin in response to deployment of the inflatable device.
3. The system of claim 1 wherein the tear seam partially penetrates the skin so that a visible surface of the skin adjacent the tear seam has a fiber matrix that is undisrupted.
4. The system of claim 3 wherein the undisrupted fiber matrix adjacent the tear seam provides a remaining wall thickness in a range of 0.2 to 0.6 mm.
5. The system of claim 1 wherein the tear seam has a strip width at the hidden surface less than or equal to 12 mm.
6. The system of claim 1 wherein the tear seam has a strip width at the hidden surface in a range of 2 to 4 mm.
7. The system of claim 1 wherein the tear seam is comprised of a dashed pattern.
8. A method of pre-weakening a tear seam on a leather cover skin for an automotive interior trim panel system, comprising the steps of: registering a leather cover skin in a substantially horizontal orientation with a hidden surface facing upward; metering an alkaline solution at a predetermined rate along a predetermined track on the hidden surface to react with the skin, thereby locally disrupting a fiber matrix of the skin to a predetermined depth to define a tear seam; and drying the skin.
9. The method of claim 8 wherein the alkaline solution has a pH in a range from 8 to 12.
10. The method of claim 9 wherein the alkaline solution is comprised of at least one of ammonia, bleach, sodium tetraborate, sodium hydroxide, sodium bicarbonate, trisodium phosphate, potassium hydroxide, and potassium carbonate.
11. The method of claim 8 wherein the alkaline solution is metered at a rate less than or equal to 36 mm.sup.3 per 10 mm length.
12. The method of claim 8 wherein the alkaline solution is metered at a rate in a range of 4 mm.sup.3 to 8 mm.sup.3 per 10 mm length.
13. The method of claim 8 wherein the alkaline solution is metered to provide a track width of less than or equal to 12 mm.
14. The method of claim 8 wherein the alkaline solution is metered to provide a track width in a range from 2 mm to 4 mm.
15. The method of claim 8 wherein the drying step includes a delay adapted to provide a reaction time to allow the alkaline solution to partially penetrate the skin so that a visible surface of the skin adjacent the tear seam has a fiber matrix that is undisrupted.
16. The method of claim 8 wherein the drying step includes blowing air along the predetermined track.
17. The method of claim 8 wherein the registering step is comprised of placing the skin on a shuttle that transports the skin to a robotic applicator, and wherein the robotic applicator includes movable nozzles for delivering the metered alkaline solution and an air jet.
18. The method of claim 17 wherein the shuttle includes a chemical sensor for contacting an unhidden surface of the skin for detecting unintended penetration of the alkaline solution through the skin.
19. The method of claim 8 further comprising the step of: mounting the skin on an interior trim panel with the hidden surface contacting the panel, wherein the panel defines a deployment aperture with a door adapted to open in response to an inflatable device deployed during a crash event, and wherein the skin is mounted with the tear seam aligned with the door.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1)
(2)
(3)
(4)
(5)
(6)
(7)
(8)
(9)
(10)
DETAILED DESCRIPTION OF PREFERRED EMBODIMENTS
(11) Referring now to
(12) Instrument panel substrate 15 defines a deployment aperture through which an air bag can deploy as a passive restraint to protect a vehicle occupant during a crash event. The deployment aperture can be an open area in substrate 15, but is more typically defined by a hidden seam 25 passing through substrate 15 along a door perimeter (breakable bridges of unremoved substrate material between the door and the substrate may be left in place are various points around the door perimeter to provide support for the structure prior to an air bag deployment). Hidden seam 25 typically extends through both substrate 15 and covering layer 16. Seam 25 has typically been formed by mechanical or laser scoring prior to attachment of chute 17. An air bag module 27 is mounted to a plurality of holes 26 in chute passageway 18. Air bag module 27 is comprised of a rigid box containing a propellant source 30 and a folded bag (not shown) that is guided via passageway 18 to door 20 upon inflation by gases from propellant source 30. Air bag module 27 includes a plurality of hooks 31 that are received in a corresponding plurality of windows 26. A fastener 32 couples air bag module 27 to a cross-car beam via a bracket.
(13) In the case of a leather cover skin for an interior trim panel having a hidden pre-weakened tear seam, the conventional seam has been formed by mechanical cutting and/or removal of a portion of the leather material from the hidden surface as shown in
(14) The production of leather for use in a cover skin involves various steps such as tanning which result in the leather being acidic, having a pH typically between about 4.5 and 5.0. Finished leather gets its thickness and strength from a fiber network layer in the form of a matrix of collagen fibrils that originate in the dermis of the original animal hide. The strength and stability of leather material is dependent upon achieving the appropriate acidity in the finished product.
(15) In the present invention, a selective application of an alkaline solution to disrupt the fiber matrix in particular regions on the hidden surface of the leather skin is used to create the desired tear seam. As shown in
(16) Exposure of a desired region of the leather skin to an alkaline solution disrupts the fiber matrix without removing any material at the tear seam. Instead, the disrupted fiber matrix at the tear seam has a reduced strength, mainly as a result of becoming brittle.
(17) A preferred technique for introducing an alkaline solution to the hidden surface of a leather skin is shown in
(18) Preferably, the alkaline solution has a pH in a range from about 8 to about 12. Almost any basic (i.e., caustic) substance can be used. For example, the alkaline solution may preferably comprise at least one of ammonia, bleach, sodium tetraborate, sodium hydroxide, sodium bicarbonate, trisodium phosphate, potassium hydroxide, and potassium carbonate in an aqueous solution. Preferably, the alkaline solution is metered at a rate less than or equal to 36 mm.sup.3 per 10 mm length, and most preferably at a rate in a range of 4 mm.sup.3 to 8 mm.sup.3 per 10 mm length.
(19)
(20) After registering leather skin 66 on shuttle 65, shuttle 65 is loaded onto a conveyor for moving skin 66 into processing booth 75. Booth 75 houses a robotic applicator system 76. After shuttle 65 has transported skin 66 into booth 75, robotic applicator system 76 activates various movable nozzles for delivering a metered alkaline solution and a drying air jet, for example. Robotic applicator system 76 includes a robotic arm 77 which supports a multiple-nozzle carriage 78. The nozzles are scanned along a predetermined track on hidden surface 68. As shown in
(21) Due to use of caustic materials, booth 75 is preferably a closed system for providing a protected environment. After an operator registers a leather skin using fixture attachments on the shuttle, the shuttle presents the leather to the robotic applicator. Based on the particular trim panel design, an appropriate alkaline solution and tear seam pattern are identified by a controller (not shown) of the robotic applicator system. Known robotic actuators and a known type of control system can be used to provide a selected alkaline solution through nozzle 81 and a drying air supply through nozzle 82. Routing head 80 is used to properly position carriage 78 during scanning.
(22) A preferred method is shown in greater detail in
(23) In step 95, drying of the skin is performed. The drying step comprises a delay having a duration adapted to enable the alkaline solution to partially penetrate the leather skin. The delay provides a reaction time necessary for the alkaline solution to disrupt the fiber matrix. With proper metering, the full amount of the caustic substance in the alkaline solution may be completely consumed. Optionally, the drying step may further include blowing an air jet along the tear seam to assist in removal of any remaining water. During processing, chemical sensors on the shuttle monitor for the appearance of any alkaline solution at the front surface of the leather skin. A skin is rejected in step 96 if alkaline solution is detected by the shuttle. If not rejected, the resulting leather skin with hidden tear seam can then be mounted on a trim panel substrate in step 97 as known in the art. For example, the leather skin may be mounted to a substrate with an intervening foam being injected between the skin and substrate.