ELECTROCHEMICAL SYSTEM, APPARATUS AND METHOD TO GENERATE METAL HYDROXIDE IN THE PRESENCE OF METAL SILICATES
20210340681 · 2021-11-04
Inventors
- Gregory Hudson RAU (Castro Valley, CA, US)
- Sadaf TAHMASEBI (Halifax, CA)
- Clive Mervyn Hugh Brereton (Richmond, CA)
- Alexandru Vasile Mezei (Peterborough, CA, US)
- Michael John KELLAND (Ottawa, CA)
Cpc classification
Y02P20/133
GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
Y02P20/151
GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
Y02E60/36
GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
C25B9/65
CHEMISTRY; METALLURGY
C25B9/23
CHEMISTRY; METALLURGY
C25B15/087
CHEMISTRY; METALLURGY
C25B15/081
CHEMISTRY; METALLURGY
Y02C20/10
GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
International classification
C25B9/23
CHEMISTRY; METALLURGY
C25B15/08
CHEMISTRY; METALLURGY
Abstract
An apparatus and method are provided for the electrochemical production of hydrogen, oxygen and metal hydroxide wherein the metal is derived from a metal silicate. The process involves the electrolysis of a metal salt solution where hydrogen and a metal hydroxide are produced at the cathode, and oxygen, or chlorine, and an acid are produced at the anode. The acid is reacted with a metal silicate producing a soluble metal salt and water that is used in turn to make solid or dissolved metal hydroxide. The net CO.sub.2 and acid gas emissions of the invention and its products may therefore be significantly reduced or turned negative.
Claims
1. An apparatus for electrochemically generating metal hydroxide, oxygen and hydrogen, the apparatus comprising: an electrolytic container having an anode, a cathode, a direct current source connected to the anode and the cathode, an electrolytic solution comprising a metal salt, the electrolytic solution disposed in said electrolytic container to undergo electrolysis when a direct current is applied, at least one ion-exchange membrane disposed in said electrolytic container between said anode and said cathode and defining a cathode region and an anode region; a second container disposed externally to said electrolytic container for holding a quantity of a solid metal silicate material, the second container being in fluid communication with said electrolytic container; means for supplying acidic solution from the anode region to said second container to effect dissolution of said solid metal silicate material and to generate a metal salt solution, wherein the solid metal silicate material, the acidic solution, and the electrolytic solution have been chosen so that: (i) the metal in the solid silicate material and the metal in said metal salt are the same; and (ii) the metal salt solution and the electrolytic solution contain said metal salt; means for supplying the metal salt solution from said second container to said electrolytic container.
2. The apparatus of claim 1 further comprising purification means configured to purify said metal salt solution, before passing the purified metal salt solution from said second container to said electrolytic container.
3. The apparatus of claim 2, wherein the purification unit is configured to remove silica and other compounds from said metal salt solution, the unit being disposed between said second container and said electrolytic container.
4. The apparatus of claim 1, comprising a cation exchange membrane and an anion exchange membrane disposed in said electrolytic container between said anode and said cathode and defining an anode region, a cathode region and a central region therebetween.
5. The apparatus of claim 1, further comprising means for removing gaseous and liquid products from the electrolytic container.
6. The apparatus from claim 1, further comprising means for removing and storing the metal hydroxide.
7. The apparatus of claim 1 where said solid metal silicate is magnesium silicate.
8. The apparatus of claim 1, further comprising means for removing an acid gas from air or a gas volume using said metal hydroxide.
9. The apparatus of claim 7, wherein the acid gas is carbon dioxide.
10. A method of generating hydrogen, an oxidative gas and a metal hydroxide for sequestering gaseous carbon dioxide or other acid gases, the method comprising the steps of: (a) supplying a direct current from an electrical source at a predetermined voltage to an electrolytic container having an anode, a cathode, an electrolyte solution comprising a metal salt, an anode region adapted to generate the oxidative gas and an acidic solution, and a cathode region adapted to generate hydrogen gas and a dissolved metal hydroxide solution, the metal in said dissolved metal hydroxide solution being derived from the electrolyte solution; (b) supplying, from a source disposed externally to the electrolytic container, a metal silicate soluble in the acidic solution; (c) removing the acidic solution from the anode region to another container outside the electrolytic container, for reacting the removed acidic solution with the metal silicate to generate a metal salt solution, wherein the metal is derived from the metal silicate; (d) reacting the metal salt solution from the step (c) with the dissolved metal hydroxide solution of the step (a) to produce a reaction solution and generate another metal hydroxide, wherein the metal in said another metal hydroxide is derived from the metal silicate; (e) separating said another metal hydroxide from the remaining reaction solution in the step (d); and (f) supplying the remaining reaction solution back to the electrolytic container for use as the electrolyte solution.
11. The method of claim 10, further comprising purifying the metal salt solution after the step (c).
12. The method of claim 10, wherein: the step (a) comprises providing the electrolyte solution comprising a soluble monovalent metal salt; and the step (c) comprises generating the metal salt solution predominantly comprising one or more metals having valency of two or higher.
13. The method of claim 12, wherein: the soluble monovalent metal salt contains ions of Na or K; and the metal derived from the metal silicate is one or more selected from the group consisting of Mg, Ca, Fe, and Cr.
14. The method of claim 10 wherein the metal silicate comprises magnesium silicate.
15. The method of claim 10, wherein the steps (d) and (e) are conducted in a reactor vessel externally to the electrolytic container.
16. The method of claim 10, wherein said metal hydroxide in the step (e) is solid metal hydroxide.
17. The method of claim 10, wherein said metal hydroxide in the step (e) is solid magnesium hydroxide.
18. The method of claim 10, further comprising using said metal hydroxide for removing an acid gas from air or a gas volume.
19. The method of claim 18, wherein the acid gas is carbon dioxide.
20. The method of claim 10, further comprising using a cation exchange membrane and an anion exchange membrane, for defining the anode region, the cathode region and a central region of the electrolytic container.
21. An apparatus for electrochemically generating metal hydroxide, oxygen and hydrogen, the apparatus comprising: an electrolytic container having an anode, a cathode, a direct current source connected to the anode and the cathode, an electrolyte solution disposed in said electrolytic container to undergo electrolysis when the direct current is applied, two ion-exchange membranes disposed in said electrolytic container between said anode and said cathode and defining a cathode region, an anode region and a central region between said anode region and said cathode region; a second container disposed externally to said electrolytic container for holding a quantity of a solid metal silicate material, the second container being in fluid communication with said electrolytic container; means for supplying acidic solution from the anode region to said second container to effect dissolution of said solid mineral silicate material and to generate a metal salt solution wherein the metal is derived from said solid metal silicate material; purification means configured to purify said metal salt solution; a hydroxide reactor in fluid communication with said electrolytic container, for precipitating low-solubility metal hydroxides whose metal is derived from the dissolution of the solid metal silicate material; and a filtering unit connected to the hydroxide reactor and configured for separating the low-solubility precipitate from a solution removed from the hydroxide reactor.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
[0050] The accompanying drawings, which constitute a part of the specification, illustrate specific embodiments of the invention and, together with the detailed description of the specific embodiments, serve to explain the principles of the invention.
[0051]
[0052]
[0053]
[0054]
[0055]
[0056]
[0057]
DETAILED DESCRIPTION OF THE EMBODIMENTS
Terminology
[0058] For convenience, a list of most frequently used terms in the application are listed below. [0059] 10: Electrolytic container, or first container [0060] 12: Anode [0061] 13: Anode region [0062] 14: Cathode [0063] 15: Cathode region [0064] 16: Source of direct current [0065] 17: Central region of the electrolytic container 10 between CEM 18 and AEM 26 [0066] 18: Cation exchange membrane (CEM) [0067] 20: Second container for holding silicate material [0068] 22: Conduit for supplying acidic solution from the anode region 13 to the second container 20 [0069] 24: Conduit for passing aqueous solution from the second container 20 back to the electrolytic container 10 [0070] 25: Conduit connection to cathode region 15 to remove hydroxides [0071] 26: Anion exchange membrane (AEM) [0072] 27: Source of metal silicate, also a metal silicate mass in
[0098] In the embodiment 100 illustrated in
[0099] A second container 20 for holding a solid metal silicate material, for example magnesium silicate material, is disposed in the proximity of and outside the electrolytic container 10, the second container 20 being in fluid communication with the electrolytic container 10 by way of a conduit 22 for supplying acidic solution from the anode region 13 to the second container 20, to effect a reaction of the acidic solution with the metal silicate material, and a conduit 24 for passing aqueous solution from the second container 20 back to the electrolytic container 10. A conduit 25 is connected to the cathode region 15 to remove metal hydroxide produced during hydrolysis from the electrolytic container 10. A source 27 of solid metal silicate is provided for replenishing the silicate content in the second container 20.
[0100] A purification unit 29 is installed on the conduit 24 for removing at least some undesirable impurities, such as silica, and certain metals, from the solution leaving the second container 20 before the purified solution is returned to the electrolytic container 10.
[0101] Unit 31 is provided to retain effluent from the cathode region 15, the effluent containing metal hydroxide, in this embodiment magnesium hydroxide, before further processing of the metal hydroxide, for example in a gas contactor 54 for acid gas removal, for example carbon dioxide removal.
[0102] Pumps, valves and control equipment are used in a known manner and not illustrated herein.
[0103] As shown in
[0104] The acid formed (e.g., H.sub.2SO.sub.4) is reacted with a mass of alkaline metal silicate, in this case MgSiO.sub.3 mineral as contained in certain rocks. This reaction occurs in a separate vessel 20. Acid solution is withdrawn from the anode chamber 13 of the electrolysis cell 10 and introduced into the vessel 20. The rate and degree of the reaction of the acid and the metal silicate can be desirably increased by using elevated temperature, agitation, mixing, stirring and/or solution recycling within the reactor vessel, treatments that would be difficult or impossible to do if the reaction were performed within the electrolysis cell. Other embodiments may simply use a pile, heap or bed of metal silicate where acid is added to the top of the metal silicate mass and by gravity allowed to travel through and react with the metal silicate mass. If the solution recovered from the reaction vessel or metal silicate mass contains a significant amount of unreacted acid solution, the solution may be returned to the vessel or mass for further contacting and reaction with the metal silicate to increase the amount of metal salts or other products produced.
[0105] The reaction between the metal silicate and the acid solution produces water and a metal salt, in the example shown, MgSO.sub.4 (
[0106] Whatever metal salt electrolyte is initially used, an important feature of this embodiment is that the anion portion of the electrolyte is mostly if not entirely conserved and recycled, while the metal cation portion of the salt electrolyte is renewed from the metal silicate.
[0107] Thus, the metal cations initially composing the electrolyte of the electrolytic container 10 are eventually replaced by metal cations derived from the metal silicate, and the metal composition of the electrolyte can therefore change over time if the initial metal cations differ from those derived from the metal silicate.
[0108] The purity of the metal salt solution formed from the reaction of the metal silicate with the acid is a concern when the resulting metal salt solution is used as an electrolyte. It is therefore desirable to avoid the presence of ions and compounds that degrade the performance of the electrolytic container 10. It may also be desirable to remove other constituents formed in the mineral/acid reaction that may have commercial value. These constituents can include but are not limited to aluminum, chromium, nickel, cobalt, iron and/or silica.
[0109] Various methods can be employed for removing such constituents from the metal salt solution prior to its use as the electrolyte in the electrolytic cell 10 (
[0110] A cation exchange membrane 18 within the electrolytic container 10 (
[0113] The balancing metal cations in the metal salt and, hence, the metal hydroxide formed can be at least one of Na, K, Ca, Mg, Al, Fe or other metals, when the metal composing the source metal silicate used: i) contains the corresponding metal, and ii) forms a soluble, dissolved salt during the metal silicate/acid reaction in the second container 20.
[0114] It is preferable that the metal silicate be crushed or ground to provide sufficient reactive surface area for contacting and reacting with the acid, and means may be needed to resupply crushed or ground metal silicate that is consumed by the process.
[0115] The anions balancing the metal cations in the metal salt can be SO.sub.4.sup.2−, PO.sub.4.sup.3−, NO.sub.3.sup.−, or other anions: [0116] i) whose pairing with the metal cations forms a metal salt that is soluble in water, and [0117] ii) whose pairing with H.sup.+ forms an acid that can react with the metal silicate to form a metal salt and water.
[0118] The use of a metal salt solution containing chloride ion, Cl.sup.−, can be used as the electrolyte if an acid of sufficient strength to dissolve metal silicate can be generated by the electrolysis of the metal chloride solution.
[0119] This can occur via the reaction of the Cl.sub.2 (now preferably discharged instead of O.sub.2 at the anode) and water to produce a mixture of hypochlorous acid, HOCI, and hydrochloric acid, HCl: Cl.sub.2+H.sub.2O--->HOCl+HCl.
[0120] HCl can also be generated by the reaction with the H.sub.2 gas produced at the cathode, and Cl.sub.2 gas produced at the anode: H.sub.2+Cl.sub.2--->2HCl.
[0121] It is also possible to use certain current densities, for example described in a paper to Bennett, J. E. Electrodes for generation of hydrogen and oxygen from seawater. Int. J. Hydrogen 1980, 5, 401-408, in the electrolytic container 10 or to use anodes 13 of certain composition, for example as describe in the paper to Bennett, 1980 cited above, to selectively discharge of O.sub.2 rather than Cl.sub.2 at the anode 13, thus allowing the H.sup.+ produced at the anode 13 to pair with the Cl.sup.− in the electrolyte to form HCl. Water of sufficient purity, such as de-ionized water, must be replenished in the electrolytic container 10 to make up for the water lost to the production of H.sub.2 and O.sub.2 and the water lost in the removal of the metal hydroxide solution from the electrolytic container 10.
[0122]
[0123] Similarly as in
[0124] In the embodiments of
MgSO.sub.4+3H.sub.2O+Vdc--->H.sub.2+0.5O.sub.2+H.sub.2SO.sub.4+Mg(OH).sub.2 (reaction 1)
H.sub.2SO.sub.4+rock/ore (containing MgSiO.sub.3 and other metal silicates and oxides)--->MgSO.sub.4+
H.sub.2O+other metal compounds+SiO.sub.2 (reaction 2)
where the MgSO.sub.4 and H.sub.2O produced in reaction 2 are then used in reaction 1. This in effect recycles the SO.sub.4.sup.2— and some water portion of the electrolyte (via 22, 24 in
[0125] A flow chart 300 of the general operation of the preceding embodiments illustrated in
[0126] The electrolytic container 10 is supplied with a soluble metal salt 42 and water 44. A direct voltage 16 is applied to the electrodes of the electrolytic container 10 resulting in the generation of oxygen 48, hydrogen 50, a metal hydroxide solution 52 and an acid solution 49. Hydrogen and oxygen gases are removed. The metal hydroxide solution 52 is removed to a container 31 (
[0127] The acid solution 49 is transferred by conduit 22 to the second container 20 (
[0128] An apparatus 400 of a third embodiment of the invention shown in
[0129] In particular, a dissolved metal salt of a monovalent metal ion is used as the electrolyte, for example Na.sup.+ or K.sup.+ as balanced by anions such as SO.sub.4.sup.2−, PO.sub.4.sup.3−, NO.sub.3.sup.− or other anions. In these cases, the metal salt as well as water are split to form H.sub.2 and a highly soluble metal hydroxide at the cathode such as NaOH or KOH, while the anion portion of the electrolyte passes through the anion exchange membrane 26 to pair with the H.sup.+ formed at the anode 12 to produce an acid, where O.sub.2 (or Cl.sub.2) is also discharged. In the example shown in
[0130] The acid solution formed in the anode region 13 is withdrawn and reacted with a metal silicate mass 27 in the second container 20 to produce a metal salt solution as previously described. Here, due to their abundance in metal silicates, divalent and higher valency metal ions, such as Mg.sup.2+, Ca.sup.2+ and Fe.sup.2+, are likely to be present in the metal salt produced in the second container 20, for example Mg.sup.2+ as shown in
[0131] Unlike embodiments 100 and 200 (
[0132] The precipitate, solid metal hydroxide formed in the reactor 34 can be further separated from the dissolved metal salt solution via flocculation followed by settling-thickening filtration, centrifugation or other solid/liquid separation methods which take place in units 36 (Settling/Filtration) and 38 (Electrolyte Cleanup) as shown in
[0133] The monovalent metal salt solution, effluent from units 36 and 38, e.g., Na.sub.2SO.sub.4 solution, is then returned to the cathode region 15 of the electrolytic container 10 to provide fresh electrolyte.
[0134] A further embodiment 500 is illustrated in
[0135] Thus, due to the provision of the reactor 34, the embodiments of
[0136] In the embodiments of
Na.sub.2SO.sub.4aq+3H.sub.2O+V.sub.dc--->H.sub.2+½O.sub.2+H.sub.2SO.sub.4aq+2NaOH.sub.aq (reaction 3)
H.sub.2SO.sub.4aq+rock (containing MgSiO.sub.3 and other metal silicates and oxides)--->MgSO.sub.4+H.sub.2O+
other metal compounds+SiO.sub.2 (reaction 4)
MgSO.sub.4aq+2NaOH.sub.aq----->Na.sub.2SO.sub.4aq+Mg(OH).sub.2s (reaction 5)
where Na.sub.2SO.sub.4aq produced in reaction 5 and the H.sub.2O produced in reaction 4 are returned to reaction 3, and Mg(OH).sub.2 is removed from solution as a solid. This in effect allows recycling of the Na.sub.2SO.sub.4aq and some water portion of the electrolyte, while forming and removing Mg(OH).sub.2 as a solid, as well as generating H.sub.2, O.sub.2, other metal compounds and silica.
[0137] In all of the preceding embodiments of
[0138] For example:
Mg.sup.2++2OH.sup.−+2CO.sub.2g---->Mg.sup.2++2HCO.sub.3.sup.− (reaction 6)
where Mg.sup.2++2OH.sup.− represents Mg(OH).sub.2 dissolved in water, i.e., Mg(OH).sub.2aq. Mg.sup.2++CO.sub.3.sup.2− (MgCO.sub.3aq) may also form via equilibrium reactions. Furthermore, MgCO.sub.3s may be formed as a solid, and may precipitate from solution. The formation of Mg(HCO.sub.3).sub.2aq, MgCO.sub.3aq and/or MgCO.sub.3, causes the original acid gas, in this case CO.sub.2, to be sequestered from the gas volume, thus desirably reducing its acid gas burden. By analogy, other metal hydroxides can be produced by the embodiments of the present invention such as Ca(OH).sub.2 and Fe(OH).sub.2, and may be used in the preceding reactions to reduce the acid gas burden in a gas volume.
[0139] When the metal hydroxide is in dissolved form, the contacting of the metal hydroxide solution and the gas volume may occur in a conventional gas/liquid contactor 54 known in the art, thus producing a metal salt of the acid gas, e.g., Mg(HCO.sub.3).sub.2aq, MgCO.sub.3aq and/or MgCO.sub.3s via reaction 6.
[0140] Similarly, when the metal hydroxide is in solid form, e.g., a Mg(OH).sub.2s, an engineered gas/solids contactor can be employed if sufficient water is supplied to dissolve some of the metal hydroxide to facilitate the formation of dissolved or solid metal salt of the acid gas, e.g., Mg(HCO.sub.3).sub.2aq, MgCO.sub.3aq and/or MgCO.sub.3s via reaction 6. To facilitate transportation and use, the mass of solid, wet, metal hydroxide particles may also be dewatered by pressure filtration, centrifuging, squeezing, heating, evaporation vacuum or other dewatering method to form a dry, metal hydroxide mass.
[0141] A flow chart 600 illustrating the possible use of metal hydroxides and (bi)carbonate in performing CO.sub.2 removal from air is shown in
[0142] When acid gas removal from air is desired, the metal hydroxide/acid gas contacting can also occur at the interface between a natural or artificial waterbody and the overlying air, wherein the produced metal hydroxide (solid or dissolved) is added to the surface waters of the waterbody, thus chemically increasing the acid gas uptake and retention by the surface waters, and drawing in and sequestering some or all of the acid gas from the overlying atmosphere, e.g., via reaction 6.
[0143] Such water bodies include but are not limited to natural ponds, lakes, rivers and oceans as well as artificial reservoirs or wastewater streams. It is desirable to keep the concentration of the added, dissolved metal hydroxide in the water body below that which causes biological or environmental harm, typically a concentration that effects a water body pH of <9, and preferably pH<8.5. Keeping chemical and biological impacts within acceptable/beneficial limits can be facilitated by dilution of the metal hydroxide(s) prior to release into a water body and/or packaging and releasing the metal hydroxide(s) in a way that limits the rate at which dissolve metal hydroxide(s) is/are added to the water body.
[0144] A further feature of the invention is that the addition of the metal hydroxide and/or metal (bi)carbonate produced therefrom may be used to beneficially elevate the pH of natural or artificial water bodies whose pH is otherwise below that deemed environmentally optimal.
[0145] For example, the metal hydroxide and/or the metal (bi)carbonate produced from it can be added to a wastewater stream whose low pH would otherwise impact the biology and chemistry of the water body receiving the wastewater stream. The produced metal hydroxide and/or produced metal salt can be added to the ocean or other natural water body for the purpose of beneficially raising the pH of the water body. The metal hydroxide and/or the metal (bi)carbonate produced from it may also be added to aquacultural systems to help control pH and to supply beneficial nutrients and elements.
[0146] The metal bicarbonate and/or carbonate or other metal salts formed via the metal hydroxide/acid gas reaction may have uses other than for sequestering acid gas or modifying water body pH, and, further, that the metal hydroxide may have uses other than for acid gas removal. These uses include but are not limited to chemical, industrial, environmental, aquacultural and agricultural uses.
[0147] The H.sub.2 and O.sub.2 produced during the electrolysis can be harvested, processed, pressurized, stored and/or used by employing methods known in the art. Alternatively, the H.sub.2 and O.sub.2 can be reacted internally within the electrochemical cell via the use of a gas diffusion electrode. This reduces the energy cost of the metal hydroxide production, but precludes H.sub.2 and O.sub.2 as marketable co-products of the system.
[0148] Thus, by combining reactions 3-6, the net electrogeochemical reaction in the preceding example is:
rock/ore (containing MgSiO.sub.3s and other metal silicates and oxides)+2H.sub.2O+2CO.sub.2g+V.sub.dc--->
H.sub.2+0.5O.sub.2+Mg(HCO.sub.3).sub.2aq+other metal compounds+SiO.sub.2 (reaction 7)
or if dissolved or solid MgCO.sub.3 is formed:
rock/ore (containing MgSiO.sub.3s and other metal silicates and oxides)+H.sub.2O+CO.sub.2g+V.sub.dc--->
H.sub.2+0.5O.sub.2+MgCO.sub.3+other metal compounds+SiO.sub.2 (reaction 8)
[0149] Metal hydroxides other than or in addition to Mg(OH).sub.2 may form due to the use of rock/ore containing metals other than or in addition to Mg and therefore that metal bicarbonates and or carbonates other than Mg(HCO.sub.3).sub.2 and MgCO.sub.3 may form upon metal hydroxide carbonation. Also, acid gases other than CO.sub.2 may participate in these reactions thus forming metal salts other than metal bicarbonate and carbonate.
[0150] A flow-chart 700 of the operation of the apparatus of
[0151] In
[0152] The acid solution 49 is transferred to the second container 20 (
[0153] In the step 92, a precipitation of solid divalent metal hydroxide 94 from a monovalent metal salt solution takes place. The precipitated hydroxide is removed at step 54 performed in the unit 36 of
Example 1
[0154] A two-compartment electrolysis cell 10 is assembled such that an anion exchange membrane 26 divides the cathode region 13 and the anode region 15. A platinized titanium or a nickel cathode 14 is inserted into the cathode region 15, and an iridium oxide coated anode 12 is inserted into the anode region 13. The anode region 13 and the cathode region 15 have inlet and outlet ports to facilitate the addition of water and electrolyte solution, and the removal of electrolysis products and any unreacted electrolyte solution.
[0155] The cathode region 15 is plumbed to a reservoir containing a 15-25% solution of Na.sub.2SO.sub.4 in de-ionized water, and the anode region 13 is plumbed to a source of de-ionized water.
[0156] The anode region 13 and the cathode region 15 are filled with the respective solutions, and a direct current electrical potential of 4-6 V.sub.dc is applied that allows for the splitting of the salt and water into hydrogen gas (H.sub.2), oxygen gas (O.sub.2), sulfuric acid (H.sub.2SO.sub.4) and sodium hydroxide (NaOH). The O.sub.2— and H.sub.2SO.sub.4— containing solution is removed from the anode region 13, and dissolved O.sub.2 is allowed to further degas from the solution and is either vented to the atmosphere or further processed for use.
[0157] De-ionized water is added to the anode region 13 to compensate for the loss of water in the formation of O.sub.2 and the removal of the H.sub.2SO.sub.4 solution. The rate of the removal of the O.sub.2+H.sub.2SO.sub.4 solution from the anode region 13 and the corresponding rate of de-ionized water addition determines the concentration of the H.sub.2SO.sub.4 solution formed, with the desired H.sub.2SO.sub.4 concentration being >7 wt. % or having a solution pH of <3.
[0158] The H.sub.2SO.sub.4 solution is pumped to the top of the second container 20 containing a mass (heap, pile or bed) of crushed rock fragments containing metal silicate minerals of the following approximate composition as an example: 38% MgO, 38% SiO.sub.2, 18% Fe, 1% CaO, 1% Al.sub.3O.sub.3, 0.2% Ni, 0.01% Cr and other constituents.
[0159] The H.sub.2SO.sub.4 solution applied to the top of the crushed rock mass flows down by gravity through and reacts with the crushed rock mass, producing sulfate salts of the metals contained in the rock mass. Those metal salts that are soluble and still contained in the solution at the bottom of the rock mass are collected at the bottom of the second container 20. The collected solution will primarily contain MgSO.sub.4aq as well as smaller quantities of other metal sulfates, any unreacted H.sub.2SO.sub.4, dissolved silica, and possibly suspended particles. The acid leaching of the crushed rock mass is allowed to progress until the rate of metal ion concentration increase levels off.
[0160] In this example, the most efficient deployment of the embodiments of the invention limits the actual extraction efficiency within a range from about 25% to 80%, preferably from 30 to 60%. This is achieved by setting the mass ratio of the H.sub.2SO.sub.4 solution and rock mass within a range from 2:1 to 6:1 preferably from 3:1 to 5:1. The molar ratio of H.sub.2SO.sub.4 supplied versus the MgSO.sub.4 formed ranges from 0.35 to 0.95, and preferably from 0.45 to 0.65. The irrigation rate of the acid solution should range from 0.08 to 0.4 liters per minute per square meter of rock mass footprint, and preferably from 0.12 to 0.28 liters/(min.×meter.sup.2).
[0161] The solution collected from the bottom of the rock mass will primarily contain MgSO.sub.4aq as well as smaller quantities of other metal sulfates, any unreacted H.sub.2SO.sub.4, dissolved silica, and possibly suspended particles.
[0162] The solution pH may then be lowered via adding additional H.sub.2SO.sub.4 solution to facilitate precipitation of solid or colloidal silica and/or other silicone-containing compounds. These compounds are filtered from the solution or removed by other means and discarded or further processed into marketable products such as silica. The remaining solution, predominantly containing MgSO.sub.4aq and smaller quantities of other dissolved metal sulfates, and possibly other compounds, is then pumped into the vessel (reactor) 34 holding a MgSO.sub.4 solution.
[0163] Meanwhile, a portion of the solution containing H.sub.2 and NaOH formed in the cathode region 15 and any unreacted Na.sub.2SO.sub.4 solution is removed from the cathode region 15. The removal rate of this solution is such that a 10 wt % or higher wt. % NaOH solution (pH>12) is formed and removed. The H.sub.2 gas is separated from the solution and the H.sub.2 gas is vented or further processed and stored for eventual use or sale.
[0164] The remaining solution, predominantly an NaOH solution is then added to a vessel 34, a reaction reservoir into which the dissolved metal sulfate solution produced in the container 20 is also added. Due to significant differences in solubility of metal ions in the presence of hydroxide ions, the less soluble divalent and higher valency metal hydroxides precipitate from solution. In this case the dominant hydroxide precipitated is Mg(OH).sub.2s, followed by lesser quantities of Fe(OH).sub.2s Ca(OH).sub.2s, Ni(OH).sub.2 and Cr(OH).sub.3s, etc.
[0165] The threshold solution pH at which these metal hydroxides precipitate differs among the metal ion species and it is therefore possible to selectively precipitate specific metal hydroxides by sequentially increasing pH. The precipitation sequence as pH rises is: Cr(OH).sub.3, Ni(OH).sub.2, Fe(OH).sub.2 Mg(OH).sub.2, and Ca(OH).sub.2. In any case, the solid metal hydroxides either separately or in bulk are then harvested from solution by filtration or other methods of liquid/solid separation. This can be preceded by adding a flocculant/coagulant such as Ca(OH).sub.2 that speeds the settling of suspended metal hydroxide particles.
[0166] The remaining solution in the vessel 34, now predominantly Na.sub.2SO.sub.4aq, is further processed before being returned to the electrolytic container 10 to function as the electrolyte (e.g.,
[0167] The moist, solid metal hydroxides, either the Mg(OH).sub.2s alone or together with the other metal hydroxides harvested as previously described, are spread on the ground (e.g., on top of the mine tailings of the mine from which the metal silicates were mined) so as to facilitate air contacting and the removal and sequestration of CO.sub.2 from the air (e.g., via reaction 6 above).
[0168] The moist, metal hydroxides may also be added to an artificial pond to elevate OH.sup.− in the pond and hence facilitate CO.sub.2 removal and sequestration from air. Likewise, the metal hydroxides may also be added to surface waters of natural water bodies like the ocean provided that the resulting chemical and biological impacts are acceptable/beneficial, in particular that pH and dissolved metal and Si concentrations do not exceed safe limits. Keeping chemical and biological impacts within acceptable/beneficial limits can be facilitated by dilution of the metal hydroxide(s) prior to release into a water body and/or packaging the metal hydroxide(s) in a way that limits the rate at which dissolve metal hydroxide(s) is/are added to the water body.
[0169] The transport of the metal hydroxides can be facilitated by dewatering the moist, metal hydroxide solids via pressure filtration, centrifuging, heat drying or other methods. Those metal hydroxides not used to facilitate CO.sub.2 removal and sequestration can be used for other purposes including refinement to reduced metals such as Fe, Ni and Cr.
Example 2
[0170] The above-described electrolysis, hydroxide production and electrolyte recycling (Example 1) can also be performed in a three-compartment cell as illustrated in
[0171] It is understood that any metalliferous compound may be used in place of the above-mentioned metal silicate if that metalliferous compound reacts with the above-mentioned acid solution to form a metal salt in solution and that metal salt solution can act as an electrolyte and/or as the source of metal hydroxide as described in the preceding embodiments. Such metalliferous compounds include but are not limited to metal carbonates and bicarbonates.
[0172] The foregoing has constituted a description of specific embodiments showing how the invention may be applied and put into use. These embodiments are only exemplary. The invention in its broadest, and more specific aspects, is further described and defined in the claims which now follow.