Construction method for ecologically protecting expansive soil slope by combining phosphogypsum with microbial mineralization

10913894 ยท 2021-02-09

Assignee

Inventors

Cpc classification

International classification

Abstract

The present invention provides a construction method for ecologically protecting an expansive soil slope by combining phosphogypsum with microbial mineralization. The method includes: (1) placing Bacillus pasteurii in a culture medium to prepare a microbial solution, and mixing urea, calcium chloride and water to prepare a cementing solution; (2) preparing a mixture with phosphogypsum fly ash and soil; mixing the mixture, the microbial solution and water well, and adding the cementing solution and water to prepare an improving mixture slurry; and (3) spraying the improving mixture slurry to a face of the slope by wet spraying, and covering with a non-woven fabric by tying and fixing.

Claims

1. A design and construction method of an expansive sol slope conditioned with phosphogypsum and a microbe, comprising the following steps: (1) preparing a culture medium and a microbial solution, wherein a mixed solute in the culture medium comprises bean pulp, (NH.sub.4).sub.2SO.sub.4, Na.sub.2HPO.sub.4 and NaOH: weighting 40 parts of bean pulp, 10 parts of (NH.sub.4).sub.2SO.sub.4, 3.55 parts of Na.sub.2HPO.sub.4 and 40 parts of NaOH by mass to prepare the mixed solute of the culture medium; mixing the mixed solute of the culture medium with water to prepare a liquid medium, the content of the bean pulp in the liquid medium being controlled at 20-60 g/L; sealing and sterilizing the liquid medium in an autoclave at 121 C. for 25 min, and then cooling to 302 C. for use; adding 1 part by volume of Bacillus pasteurii solution to 100 parts by volume of liquid medium to prepare the microbial solution; placing the microbial solution into a constant-temperature shaking incubator at 30 C., and shaking at 200 rpm for more than 24 h until an optical density of the microbe in the microbial solution at a wavelength of 600 nm (OD.sub.600) is 1.50.2; (2) preparing a cementing solution, wherein a mixed solute in the cementing solution comprises urea and calcium chloride: weighing 2 parts of granular urea and 1 part of powdered calcium chloride by mass to prepare the mixed solute, and mixing the mixed solute with water to prepare the cementing solution with a concentration of 0.50.1 mol; (3) preparing a mixture comprising phosphogypsum, fly ash and soil: weighing 19 parts of phosphogypsum, 1 part of fly ash and 40-50 parts of sod by dry mass, and mixing well to the mixture, wherein the soil in the mixture is expansive soil, loam or planting soil; (4) preparing an improving mixture slurry: weighing 100-1,000 pans of mixture, 1 part of microbial solution and 10 parts of cementing solution by volume; first mixing the 100-1,000 parts of mixture and 1 part of microbial solution with water well; then adding the 10 parts of cementing solution and water, and mixing well to obtain the improving mixture slurry, wherein the microbial solution and the cementing solution are each added once in the whole process; (5) laying a three-dimensional vegetation net: leveling an excavated slope; constructing an intercepting ditch on a crest of the slope, a drainage ditch on a toe of the slope and a drainage groove on a face of the slope; laying the three-dimensional vegetation net on the face of the slope from top to bottom, and fixing the three-dimensional vegetation net, wherein the three-dimensional vegetation net extends 40-80 cm on the crest of the slope to be buried in the soil and compacted; a longitudinal/transverse tensile strength of the three-dimensional vegetation net is greater than 1.0 kN/m; and (6) spraying and sowing: spraying the improving mixture slurry by wet spraying to the face of the slope twice from top to bottom and left to right with a thickness of 41 cm each; then mixing the improving mixture slurry with grass seeds well, and spraying to the face of the slope once, wherein the spraying thickness is 41 cm, and the total thickness of the sprayed improving mixture slurry on the face of the slope is not less than 10 cm; not less than 25 g of grass seeds are sown per square meter of the face of the slope; the prepared improving mixture slurry is sprayed to the face of the slope in 6 h; then covering with a non-woven fabric by tying and fixing to the slope, and watering every day.

Description

BRIEF DESCRIPTION OF THE DRAWINGS

(1) FIG. 1 is a schematic elevation view of a slope paved with a three-dimensional vegetation net, wherein numeral 1 refers to intercepting ditch, numeral 2 refers to drainage ditch, numeral 3 refers to drainage groove and numeral 4 refers to three-dimensional vegetation network.

(2) FIG. 2 is a schematic cross-sectional view of AA in FIG. 1, wherein numeral 1 refers to intercepting ditch, numeral 2 refers to drainage ditch, and numeral 4 refers to three-dimensional vegetation network.

DETAILED DESCRIPTION

(3) Example: a construction method for ecologically protecting an expansive soil slope by combining phosphogypsum with microbial mineralization, including the following steps:

(4) (1) Prepare a culture medium and a microbial solution: weigh 8 kg of bean pulp, 2 kg of (NH.sub.4).sub.2SO.sub.4, 0.71 kg of Na.sub.2HPO.sub.4 and 8 kg of NaOH to prepare a mixed solute of the culture medium; mix the mixed solute of the culture medium with 200 kg of water to prepare a liquid medium; seal and sterilize the liquid medium in an autoclave at 121 C. for 25 min, and then cool to 30 C. for use; add 2 L of Bacillus pasteurii solution to the liquid medium to prepare the microbial solution; place the microbial solution into a constant-temperature shaking incubator at 30 C., and shake at 200 rpm for more than 24 h until an optical density of the Bacillus pasteurii in the microbial solution at a wavelength of 600 nm (OD.sub.600) is 1.5.

(5) (2) Prepare a cementing solution: weigh 240 kg of urea and 120 kg of calcium chloride, mix with water to prepare 2,020 L of cementing solution with a concentration of 0.5 mol.

(6) (3) Prepare a mixture: weigh 43.0 t of phosphogypsum, 2.2 t of alkaline slag and 106.2 t of loam, and mix well to obtain the mixture.

(7) (4) Prepare an improving mixture slurry: mix 101.0 m.sup.3 of mixture, 0.2 m.sup.3 of microbial solution and 20 m.sup.3 of water well; then add 2 m.sup.3 of cementing solution and 8 m.sup.3 of water, and mix well to obtain the improving mixture slurry, where the mixture has a bulk density of 1.5 g/cm.sup.3.

(8) (5) Slope protection: With reference to FIGS. 1-2, level an excavated slope; construct an intercepting ditch 1 on a crest of the slope, a drainage ditch 2 on a toe of the slope and a drainage groove 3 on a face of the slope: lay a three-dimensional vegetation net 4; spray the improving mixture slurry by wet spraying to the face of the slope twice front top to bottom and left to right with a thickness of 4 cm each; then mix the improving mixture slurry with grass seeds well, and spray to the face of the slope once with a thickness of 3 cm; then cover with a non-woven fabric by tying and fixing, and water every day.