Protecting anodes from passivation in alloy plating systems
10954605 ยท 2021-03-23
Assignee
Inventors
- Lee Peng Chua (Beaverton, OR)
- Steven T. Mayer (Aurora, OR)
- David W. Porter (Sherwood, OR)
- Thomas A. Ponnuswamy (Sherwood, OR)
Cpc classification
C25D17/001
CHEMISTRY; METALLURGY
C25D5/00
CHEMISTRY; METALLURGY
C25D17/002
CHEMISTRY; METALLURGY
C25D17/10
CHEMISTRY; METALLURGY
International classification
C25D17/00
CHEMISTRY; METALLURGY
C25D17/10
CHEMISTRY; METALLURGY
Abstract
An apparatus for continuous simultaneous electroplating of two metals having substantially different standard electrodeposition potentials (e.g., for deposition of SnAg alloys) comprises an anode chamber for containing an anolyte comprising ions of a first, less noble metal, (e.g., tin), but not of a second, more noble, metal (e.g., silver) and an active anode; a cathode chamber for containing catholyte including ions of a first metal (e.g., tin), ions of a second, more noble, metal (e.g., silver), and the substrate; a separation structure positioned between the anode chamber and the cathode chamber, where the separation structure substantially prevents transfer of more noble metal from catholyte to the anolyte; and fluidic features and an associated controller coupled to the apparatus and configured to perform continuous electroplating, while maintaining substantially constant concentrations of plating bath components for extended periods of use.
Claims
1. A leak detection probe comprising: a first electrode comprising substantially tin metal; a second electrode comprising substantially a second metal more noble than tin; and an electrically insulating separator positioned between the first electrode and the second electrode, wherein the leak detection probe is configured to detect presence of metal ions in a tin ion containing electrolyte, wherein the metal ions are of a metal more noble than tin, and wherein the leak detection probe is further configured such that the first and the second electrode both contact the same tin ion containing electrolyte and such that the tin ion containing electrolyte flows through the electrically insulating separator and contacts the second electrode during operation.
2. The leak detection probe of claim 1, further comprising a resistor electrically connecting the first electrode and the second electrode, wherein the leak detection probe is configured such that voltage across the resistor is used to detect the presence of the metal ions in the tin ion containing electrolyte.
3. The leak detection probe of claim 1, wherein the second metal is porous silver.
4. The leak detection probe of claim 1, wherein the first electrode is a rod centrally disposed in the leak detection probe, wherein the electrically insulating separator is disposed around at least a portion of the perimeter of the rod, and wherein the second electrode is disposed around at least a portion of an outer perimeter of the electrically insulating separator.
5. The leak detection probe of claim 4, further comprising a sense lead connected to the second electrode.
6. The leak detection probe of claim 1, wherein the probe has an impedance of between about 10 ohm and 1 ohm.
7. The leak detection probe of claim 1, wherein the first electrode comprises low alpha tin.
8. The leak detection probe of claim 1, wherein the metal ions detected in the tin ion containing electrolyte are silver ions.
9. The leak detection probe of claim 1, wherein the electrically insulating separator comprises an electrolyte permeable membrane.
10. The leak detection probe of claim 1, wherein the electrically insulating separator comprises an electrolyte permeable sintered glass or plastic.
11. The leak detection probe of claim 1, wherein the first and second electrodes are electrically connected to a power supply.
12. The leak detection probe of claim 1, wherein the first and second electrodes are electrically connected to a power supply that is configured to positively bias the second electrode relative to the first electrode.
13. The leak detection probe of claim 12, wherein the power supply is configured to maintain a potential between leads to the first and second electrodes at a fixed value.
14. The leak detection probe of claim 1, wherein the second electrode is a silver foil electrode.
15. The leak detection probe of claim 1, wherein the second electrode comprises sintered silver powder.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1)
(2)
(3)
(4)
(5)
(6)
(7)
(8)
(9)
(10)
(11)
(12)
(13)
(14)
DETAILED DESCRIPTION
Introduction
(15) In alloy electroplating systems, where one or more of the metal species has a significantly different reduction potential than another metal species, such as in SnAg (tin-silver) solder electroplating, formidable challenges exist in implementing a design employing an active anode (i.e., and metal anode that dissolves during electroplating). One of these challenges is an exchange/displacement reaction resulting in anode surface passivation. For example, the passivation of an anode having a significantly less noble metal (e.g., tin) may occur by the following displacement reaction, Sn(s)+2Ag.sup.+.fwdarw.Sn.sup.2++2Ag(s), which, due to the large reduction potential differences of tin and silver, can occur quite readily. If silver coats the tin anode surface, it may make passage of current significantly more difficult and non-uniform. It may also generate unwanted particles, etc.
(16) The present disclosure pertains to methods and apparatus using gettering to remove or getter unwanted reactive cations, Ag.sup.+ in one embodiment, from a separated anode chamber (SAC), where the tin anode is housed. In a particular embodiment, the SAC compartment is substantially free of the more noble metal (e.g. silver) and separated from the cathode chamber containing catholyte. As explained below, the separation is typically accomplished by the using a cationic membrane whose properties provide a partial or nearly complete exclusion of noble metal from separated anode chamber. However, because perfect separation cannot always be ensured and because small leaks in the sealing members may occur, gettering is used to remove Ag.sup.+ ions from the anolyte in a substantially continuous fashion, hence freeing or reducing the aforementioned passivation and other issues.
(17) The disclosure also concerns an in-situ method of detecting Ag.sup.+ contamination in the SAC compartment, which increases the reliability and robustness of the system and can be used to warn and thereby prevent the plating tool from running high value product wafer after a potential leak or some other source of contamination isolation failure between the two chambers.
(18) Generally, the methods and apparatus provided herein are suitable for simultaneous electrodeposition of at least two metals having different electrodeposition potentials. These methods are particularly suited to depositing metals having a large difference in standard electrodeposition potentials, such as a difference of at least about 0.3 V, or at least about 0.5 V or more. These methods and apparatus will be illustrated using simultaneous electrodeposition of tin (less noble metal) and silver (more noble metal) as an example. The standard electrochemical potentials (E.sub.0s) of tin and silver are separated by more than 0.9 volts (Ag.sup.+/Ag: 0.8V NHE, Sn.sup.+2/Sn: 0.15V). Stated another way, elemental silver is substantially more inert than elemental tin and therefore will electroplate out of solution first much more easily than tin.
(19) It is understood that the provided apparatus and methods can also be used for simultaneous electrodeposition of other metal combinations (including alloys and mixtures), such as combinations of tin and copper, nickel and silver, copper and silver, indium and silver, iron and nickel, gold and indium, or two metal micro-mixtures such as gold and copper or copper and nickel. Electrodeposition of more than two metals can also be accomplished. For example, known ternary lead free alloys of tin, copper and silver, can be electrodeposited using methods and apparatus provided herein.
(20) It is noteworthy that in some embodiments, low alpha tin is employed in the plating systems provided herein as a less noble metal. Low alpha tin is tin of extremely high chemical purity with low levels of alpha particle emitted (e.g. less than about 0.02 alpha emission counts per cm.sup.2 per hour, or less than about 0.002 alpha emission counts per cm.sup.2 per hour). This is significant for IC applications, because alpha emission in the semiconductor chips can cause reliability problems and can interfere with IC function. Accordingly, in some embodiments, the tin anode that is used in the provided apparatus contains low alpha tin. Further, in some embodiments, the electrolyte employs stannous ions that are low alpha tin grade. Low alpha tin in solution is a more expensive material (weight for weight) than metallic low alpha tin.
(21) Electrochemical deposition may be employed at various points in the integrated circuit (IC) fabrication and packaging processes. At the IC chip level, damascene features are created by electrodepositing copper within vias and trenches to form multiple interconnected metallization layers. Above the multiple metallization layers, the packaging of the chip begins. Various wafer level packaging (WLP) structures may be employed, some of which contain alloys or other combinations of two or more metals or other components. For example, the packaging may include one or more bumps made from solder or related materials.
(22) In a typical example of plated bump manufacturing, the processing starts with a substrate having a conductive seed layer (e.g., a copper seed layer) having an underbump diffusion barrier layer of plated nickel (e.g. about 1-2 m thick and 100 m wide) under a film of lead tin solder plated pillar (e.g., 50 to 100 microns thick and 100 microns wide). In accordance with certain methods provided herein the solder pillar is made of electrodeposited tin silver instead of lead tin. After plating, photoresist stripping, and etching of the conductive substrate copper seed layer, the pillars of solder are carefully melted or reflowed to create a solder bumps or balls attached to the underbump metal. An underbump of a non-solder high melting point plated metal solder pedestal such as copper, nickel, or a layered combination of these two, is often created below a solder film. In some processes, the pedestals are replaced with smaller and higher aspect ratio pillars of the high melting metals (e.g., nickel and/or copper) resulting in reduced use of solder. In this scheme, which is useful in achieving tight and precise feature pitch and separation control, the copper pillars may be, for example, 50 microns or less in width. Features can be separated from one another by 75-100 micron center to center, and the copper may be 20-40 microns in height. On top of the copper pillar, a nickel barrier film, e.g., about 1-2 microns thick, is sometimes deposited to separate the copper from the tin-containing solder and thereby avoid a solid state reaction of copper and tin which results in formation of various undesirable bronzes. Finally, a solder layer (conventionally a SnPb layer, but a SnAg layer according to certain embodiments) typically 20-40 microns in thickness is deposited. This scheme also enables a use of reduced amount of solder for the same feature sizes, reducing the cost of solder or reducing the total amount of lead in the chip. Recently, a move away from lead-containing solders has increased in momentum due to environmental and health safety concerns. Tin-silver solder alloy bumps are of particular interest and are used as an example to describe various embodiments described herein.
(23) In chip and wafer level packaging, one method for forming the solder bumps is done by through-resist electroplating (other methods, typically now only used for larger features size/scales and prior device generations, include solder ball placement and slurry screen-paste-printing). Driven by the international lead-free industrial and environmental requirements, the industry has converged primarily to SnAg alloy solder material for electroplating lead free solders, usually at a composition close to the eutectic. The eutectic composition of silver in tin is at about 3.7 wt % silver, and, for example, typical compositions in use are between about 1.7-2.5% silver by weight. Thermodynamically, the eutectic alloy segregates into two phases, a silver rich phase (Ag.sub.3Sn) and a nearly pure tin phase.
(24) Due to the large difference in electrochemical reduction potential between tin and silver ions to pure metals, an active anode of a single metal (e.g., Sn) cannot be easily employed, at least in the conventional means of simply having a tin anode, because Ag.sup.+ ions in the bath will very readily react with the tin anode: 2Ag.sup.++Sn(s).fwdarw.2Ag(s)+Sn.sup.2+, leading to (1) continuous depletion of silver ions in the bath, and associated stability issues (continual loss of Ag.sup.+ and some small corresponding rise in Sn.sup.2+) and, (2) anode passivation as the anodes become covered by Ag(s) material.
(25) It has been seen that initially pure tin shot anodes changes appearance after being exposed to Ag.sup.+. In one case, the silver was complexed and in another the silver was substantially uncomplexed (silver in a methane sulphonic acid solution without an additional complexing agent). The silver complexer used in this example was commercially available SLG (silver-ligand), at a concentration of about 120 ml/L. available from Mitsubishi Materials Corporation of Japan. Similar results are expected with various known thiol and dithiol compounds that serve as silver complexing agents. Examples of such known compounds include 3,6-dithiaoctane-1,8-diol. As observed, a black layer of film and sludge-slime material forms around the anode depending on conditions. In the presence of the complexer, the tin anode still reacts with the silver, however, the solution tends to not change color as significantly than when the complexer is present (yellowish, possibly indicating a reaction of the free silver in the solution or the container walls with stannous ion to form stannic ion). Both factors will eventually lead to poor on wafer performance, drift, degradation, and impractical short operational life. As a result, tin silver alloy electroplating systems commonly use of an inert anode design which decomposes the water in the electrolyte to form oxygen and release acid (protons).
(26) The inert anode comes with certain disadvantages. Because tin is plated but is not generated at the anode, the inert anode design depletes tin from the solution, and therefore requires significant replenishment of Sn.sup.2+ from liquid tin containing electrolyte (dosing) as compared to an active anode system (disclosed herein and also described in U.S. Pat. No. 9,404,194, issued on Aug. 2, 2016, titled ELECTROPLATING APPARATUS AND PROCESS FOR WAFER LEVEL PACKAGING, which is incorporated herein by reference for its disclosure of an active anode system for plating two metals).
(27) Without going into extensive detail, Sn.sup.2+ dosing in the inert anode configuration arises from the need to replenish the tin metal that has been plated-out on the wafer and from significant bleed and feed operation, required to maintain the bath at a constant concentration of its various constituents. Bleed and feed is necessitated by the fact that inert anode systems generate by-product acidic protons, and bath bleeding can control the bath acid concentration level. Unfortunately, the various components of the SnAg electroplating electrolyte are costly, due in large measure to the high cost of the low alpha tin electrolyte. The overall high cost is not due just to the sheer quantity of consumed electrolyte material, but also the particular type of tin (low alpha tin) required in electronics application. As explained, high energy alpha particles, from isotopes found even in trace amount in the manufactured tin, can lead to device soft errors. Therefore, the semiconductor chip making industry requires that the tin used must be of low level alpha grade to avoid chip performance reliability issues from the aforementioned alpha-particle-induced soft errors. In addition to the chemical balance issues noted above, inert anodes systems also have the issue of oxygen gas generation at the inert anode and the need to remove the bubbles from the plating reactor and blocking bubbles from reaching the wafer surface. Also, the continual introduction of oxygen into the system heightens the risk of forming SnO.sub.2, also known in the industry as stannic sludge. The later can lead to void defects in the solder bump formation, and weakened interfacial adhesion between the solder bump and the underlying metal layer. Finally, the potential magnitude of the oxygen evolving inert anode is very high, leading to the oxidation of bath additives and silver complexers, as well as direct oxidation of stannous to stannic form of tin, and other issues. Hence in an inert anode system, bath stability and life is shortened, which further adds to operational cost and reduces available up time.
(28) In certain disclosed designs employing SnAg active anode systems 201 as depicted in
(29) Although the membrane 207 can allow diffusion, osmosis and electro-osmosis or water transport, it prohibits motion of anions while selectively permitting transport of positive charged cationic species (H.sub.3O.sup.+, M.sup.+, where M=Metal). The transport of metal cations across the membrane is generally substantially more restrictive compared to the transport of much smaller cations, particularly acid protons (H+ and H.sub.3O.sup.+). The cationic transport rate across the membrane depends on the mechanism or mode, namely (1) concentration gradient driven diffusion and (2) ionic mobility and current induced electro-migration. Migration occurs primarily during electroplating (though a diffusion or junction potential which can create an electric field under special circumstances), and is typically the overwhelmingly faster process for cationic species transport at that time, with positive ions moving in the direction from the anode in the SAC to the catholytic chamber and eventually to the wafer surface. However, during periods of no plating (idle), the remaining mode of specie transport becomes operative (diffusion). Diffusion of the highly mobile acid proton (typically 10 the mobility and diffusion coefficient of a metal ion) and less mobile metal cations across the membrane are somewhat impeded by the need to move through the membrane pores. The cationic membrane prohibits movement of free anions through it and within it. In contrast, the cationic membrane has anions which are bound or tethered as anchored sulphonate groups tied to the fluropolymer backbone change (in the case of Nafion). To maintain charge neutrality inside the membrane matrix, the motion of cations is believed to occur by a series of atomic hops or jumps of the cationic in sequential formation and breaking of negative-positive pairs. This process generally hinders the diffusion process, since a higher activation energy for the transport process is required. Therefore, even a relative thin cation membrane can introduce a significantly transport resistance to cation diffusion and mixing across the catholyte to anolyte barrier. Protons, with their small size and high mobility can move more rapidly, but because anions do not accompany the transport across the barrier and charge neutrality must be maintained (otherwise increasing the free energy due to charge separation, an unsustainable process), either another proton must move in the opposite direction, or a slower more kinetically hindered metal ion must transfer through the interface. In practice, the total ionic strength (total moles of cations+anions) of each of the two sub-system are largely immutable and would remain at that ionic strength save the diffusive motion of neutral species, particularly water (which is highly mobile across the water-swelled polymers). When the two chambers have differing total ionic strengths, water will, by diffusion and osmotic forces, move to dilute the chamber with the higher salt content (total ionic strength).
(30) The above discussion assumes that there is no physical flow (convection) through the membrane itself. This is a reasonable assumption due to the very small (atomic-size) pores within the membranes and the very high viscous forces needed to cause bulk flow. Primarily only under extremely high pressures (100-1000's of psi and more) will significant flow of materials through the membrane occur, and even in that case, most of the transport will be of neutral water (reverse osmosis) because salts are still bound by electro-neutrality.
(31) Because typical cationic membrane materials are not thermoplastics and are not plastic-weldable, O-ring and gasket seals 215 (often double, or sequential seals) are employed along the membrane sealing interfaces including the various SAC compartment sealing interfaces to ensure hermetic sealing and prevent gross leakage paths, thereby avoiding the possibility of bulk Ag.sup.+ transporting from the catholyte into the SAC compartment. However, in practice, maintaining and setting up the SAC compartment to be hermetically sealed is not always guaranteed or practical. Damage from handling and imperfect machining surfaces can also lead to minute opening and gaps allowing flow or bypassing-diffusion leak paths 217 transporting Ag.sup.+ from the catholyte chamber 219 around the membrane to the SAC compartment 205.
(32) In certain embodiments, the cathode containing chamber is outfitted with channeled ionically resistive plate 213 that facilitates uniform plating over the face of the cathodic substrate. Plate 213 provides a relatively uniform current distribution over the plating face of the substrate and strong convection at the plating face. Plate 213 may contain through-holes that are spatially and ionically isolated from each other and do not form interconnecting channels within the body of plate. As an example, plate 213 is a disc made of an ionically resistive material, such as polyethylene, polypropylene, polyvinylidene difluoride (PVDF), polytetrafluoroethylene, polysulphone, polyvinyl chloride (PVC), polycarbonate, and the like, having between about 6,000-12,000 non-communicating through-holes. The plate, in many embodiments, is substantially coextensive with the wafer substrate (e.g., has a diameter of about 450 mm when used with a 450 mm wafer) and resides in close proximity of the wafer, e.g., just below the wafer in a wafer-facing-down electroplating apparatus. In certain embodiments, the plated surface of the wafer resides within about 10 mm, or within about 5 mm of the closest plate surface. Channeled ionically resistive plates and there applications are presented in U.S. Pat. No. 9,624,592, issued on Apr. 18, 2017, and titled CROSS FLOW MANIFOLD FOR ELECTROPLATING APPARATUS, which is incorporated herein by reference in its entirety.
(33) In one embodiment, the pressure in the separated anode chamber is always slightly higher than the pressure above the membrane. This is accomplished, for example, by having a pneumatic anode chamber fluid flowing-outlet pressure regulating device (sometime referred to as the SAC fountain) that is vented to atmosphere at a level above the top surface of the fluid in the catholyte chamber, thereby maintaining a static pressure on the membrane at all times and, in the event of a small leak, having fluid flow from the SAC compartment to the catholyte chamber. This configuration makes the bulk flow of fluid through the leak path be in the direction opposite that of any diffusion into the SAC. Refer to U.S. Pat. No. 8,603,305, issued on Dec. 10, 2013 titled ELECTROLYTE LOOP FOR PRESSURE REGULATION FOR SEPARATED ANODE CHAMBER OF ELECTROPLATING SYSTEM (and incorporated herein by reference in its entirety) for more details about this embodiment.
(34) Despite on-going effort in design and process, and even with a perfect seal or having a slow flow forced backwards though a small leaking seals, diffusion of some Ag.sup.+ across the membrane, albeit however slow, may still occur. Over time, there is a risk for the SAC compartment will become contaminated with unwanted Ag.sup.+, leading to continuous reaction of silver with the less noble pure tin anode. The associated spontaneous displacement reaction may in some way coat the tin anode with a film of silver of Ag.sub.3Sn, and such a film my slowly lead to inhibition of the dissolution of tin metal, otherwise colloquially referred to as anode passivation. Therefore, this remains an open issue and a potential risk factor for one using an active anode.
(35) In the event of Ag.sup.+leaking into the SAC compartment, it can be reasoned that passivation of the anode may occur non-uniformly over the surface, or, in the case of a porous anode composed of a pile of anode spheres or slugs, non-uniformly in the depth of the anode. Generally, the upper surface of any anode is ohmically preferred to undergo reaction, and any lower surfaces or shadowed sphere not yet exposed for use, are largely electrochemically inactive until the metal anode closer to the cathode has been corroded and utilized. Therefore, for a porous anode, exposure of the surfaces to silver contamination may occur over a period of weeks or even months before that portion of the anode is actually used, at which time, the amount of displaced silver may be non-uniformly deposited on the tin interface. This non-uniform film coverage can lead to selective passivation, because, on application of current, initial the silver and Ag.sub.3Sn film we be removed uniformly, but require a higher potential than that of pure tin. Once one location (e.g. the centrally located region of the anode) has completely corroded of the silver rich film, the potential for dissolution there drops. Because the anode as a whole is electrically tied and can exert only a single potential, the potential of the anode as a whole will drop, the silver free portion of the anode will carry a disproportionately greater current density, and the uniformity of the plated film on the wafer will suffer. As a result, on wafer performance and the cell's behavior will begin to drift out of specifications once the anode becomes un-uniformly and/or sufficiently passivated. Without silver displacement reaction mitigation and/or detection in place, the robustness of a plating process cannot be assured, and may vary from wafer to wafer and over time significantly, leading to reduced repeatability and low predictability from tool-to-tool and setup-to-setup, as long as the inherent risk of anode passivation remains.
(36) A discussion of suitable apparatus, anolyte and catholyte compositions, and continuous plating methods is found in U.S. patent application Ser. No. 13/305,384 (published as US20120138471A1), previously incorporated herein by reference in its entirety.
(37) As explained, a plating cell may contain a cathode chamber 219 configured for holding catholyte and a substrate (which is cathodically biased during plating) and an anode chamber configured for holding anolyte and the anode, where the anode chamber 205 and the cathode chamber 219 are separated by a separation structure, and where the anolyte contained in the anode chamber is substantially free of metal ions of the nobler metal. In some embodiments the anolyte is also substantially free of plating bath additives such as grain refiners, brighteners, levelers, suppressors, and noble metal complexing agents. The anolyte is electrolyte that contacts the anode and has a composition appropriate for contacting the anode and allowing it to create a soluble anode metal species upon electrochemical dissolution of the anode. In the case of tin, the suitable anolyte may be highly acidic (preferably with pH of less than 2) and/or contain a tin complexing agent (e.g. a chelator such as an oxalate anion). Conversely, the catholyte is electrolyte that contacts the cathode and has a composition appropriate for that role. For tin/silver plating, one exemplary catholyte contains acid (e.g., methanesulfonic acid), a salt of tin (e.g., tin methanesulfonate), silver complexed with a silver complexer (e.g., silver complex with a thiol-containing complexer such as 3,6-dithiaoctane-1,8-diol), and a grain refiner (e.g. polyethyleneglycol (PEG), hydroxylated cellulose, gelatin, peptone, etc.). The separator helps maintain the distinct compositions of the anolyte and the catholyte within the electroplating chamber, even during electroplating, by selectively excluding certain electrolyte components from passage through the separator. For example, the separator can prevent the ions of a nobler metal from flowing from catholyte to anolyte. The term flow as used herein encompasses all types of ion movement.
(38) The following principles can be employed in designing an electroplating apparatus and/or process suitable for plating a composition containing a more noble element and a less noble element: (1) the less noble element is provided in the anode chamber, (2) a soluble compound of the more noble element (e.g., a salt of that element, often in a complexed form) is blocked from transport from the cathode chamber to the anode chamber, e.g., by the separator and (3) the soluble compound of the more noble element is applied to the cathode chamber only (not to the anode chamber). In certain embodiments, the less noble element is provided at least via a consumable anode containing that element (and can be also provided in solution in addition to consumable anode), which is electrochemically dissolved during plating.
(39) An example of a suitable apparatus for plating in accordance with embodiments provided herein is schematically illustrated in
(40)
(41) In the apparatus 100, an anode 110, which is a consumable tin anode, is typically located in a lower region of the plating cell 105. A semiconductor wafer (or other work piece) 115 is positioned in catholyte retained in the catholyte chamber 125 and is rotated during plating by a wafer holder 120. Rotation can be bidirectional. In the depicted embodiment the plating cell 105 has a lid 121 over the cathode chamber. The semiconductor wafer is electrically connected to a power supply (not shown) and is negatively biased during electroplating, such that it serves as a cathode. The active tin anode is connected to the positive terminal of the power supply. A separator 150 which is at a minimum cationically conductive for protons and inhibits direct fluid flow transfer between the anolyte and catholyte chambers, is located between the anode and the wafer (the cathode) as it separates and defines an anode chamber 145 and a cathode chamber 125. As explained, the isolated anodic region of the plating cell is often referred to as a Separated Anode Chamber (SAC). An electroplating apparatus having a SAC is described in detail in U.S. Pat. No. 6,527,920 issued on Mar. 4, 2003 to Mayer et al., U.S. Pat. No. 6,890,416 issued on May 10, 2005 to Mayer et. al., and U.S. Pat. No. 6,821,407 issued Nov. 23, 2004 to Reid et al., which are herein incorporated by reference in their entireties.
(42) Separator 150 allows selective cationic communication between the separated anode chamber and the cathode chamber, while preventing any particles generated at the anode from entering the proximity of the wafer and contaminating it. The separator, as mentioned, allows flow of protons, from anolyte to catholyte during plating. Further, the separator may allow passage of water from anolyte to catholyte, which moves along with the protons. In some embodiments, the separator is also permeable to tin ions during plating, where the tin ions will move from anolyte to catholyte, when potential difference is applied (but not in the absence of potential difference). The separator may also be useful in prohibiting anionic and non-ionic species such as bath additives from passing though the separator and being degraded at the anode surface, and as such, in some embodiments, the anolyte contained in the anode chamber remains substantially free of organic additive species (such as accelerators, levelers, suppressors, grain refiners, and silver complexers) present in the catholyte that are used to control within wafer, within die or within feature uniformity or various metrological properties.
(43) The separator having these properties can include an ionomer, e.g., a cationic polyfluorinated polymer having sulphonate groups, such as the commercially available product made by DuPont de Nemours provided under the trade name Nafion or VaNaDION from Ion Power of New Castle Del. The ionomer can be mechanically reinforced, e.g., by incorporation of reinforcing fibers within the ionomer membrane, or externally by a mechanical construct, and can reside on a mechanically strong support such as a solid material with drilled holes to create a reticulated structure, or a continuously sintered microporous material, e.g., a microporous sheet material such as Porex.
(44) In the embodiment depicted in
(45) The apparatus (in both embodiments shown in
(46) The apparatus further contains fluidic features configured to add acid and stannous ion to the anolyte. Addition of acid and stannous ion can be accomplished at any desired pointdirectly to the anode chamber, to the lines of the anolyte circulation loop, or to the pressure regulator, as depicted in
(47) The apparatus further includes a fluidic conduit 159, configured for delivering anolyte containing acid and stannous ion from the anode chamber to the cathode chamber or to the reservoir 190 containing surplus catholyte (in the embodiment of
(48) The cathode chamber of the apparatus, depicted in the embodiments shown in
(49) Further, the apparatus includes an outlet in the cathode chamber and associated fluidic features 161, configured to remove a portion of the catholyte from the cathode chamber. This stream is referred to as a bleed stream and typically contains silver ions, tin ions, acid, complexer and additives (such as grain refiners, brighteners, suppressors, accelerator and leveler). This stream is significant for maintaining overall mass and volume balance of the plating cell. In the embodiment depicted in
(50) Fluidic features, referred to herein, may include but are not limited to fluid conduits (including lines and weirs), fluid inlets, fluid outlets, valves, level sensors and flow meters. As can be appreciated, any of the valves may include manual valves, air controlled valves, needle valves, electronically controlled valves, bleed valves and/or any other suitable type of valve.
(51) A controller 170 is coupled to the apparatus and is configured to control all aspects of plating including parameters of feeding anolyte and catholyte, bleeding the catholyte, delivering anolyte to catholyte, etc. Specifically the controller is configured to monitor and control parameters (e.g. current, charge passed, bath levels, flow rates, and timing of dosing) related to need for addition of acid to anolyte, stannous ions to anolyte, water to anolyte, silver ions to catholyte, additive to the catholyte, complexer to the catholyte, delivery of anolyte to catholyte, and of bleeding (removal) of catholyte.
(52) The controller can be configured for coulometric control of the plating process. For example, bleed-and-feed and cascading can be controlled, based on the amount of Coulombs passed through the system. In specific examples, dosing of acid, and stannous ion to anolyte, dosing of silver to catholyte, cascading of anolyte to catholyte, and bleed from the catholyte can be initiated after a pre-determined number of Coulombs passed through the system. In some embodiments, these are controlled, in response to pre-determined time that has elapsed, or in response to the number of substrates processed. In some embodiments, dosing of water to compensate for evaporation is made periodically (feed forward time based) and/or in a feedback mode based on changes in measured bath volume.
(53) In some embodiments, the controller is also configured to adjust parameters of the system (such as flow rates in the mentioned streams, and timing of dosing) in response to feedback signals received from the system. For example, concentrations of plating bath components can be monitored in anolyte and/or catholyte using a variety of sensors and titrations (e.g., pH sensors, voltammetry, acid or chemical titrations, spectrophotometric sensors, conductivity sensors, density sensors, etc.). In some embodiments the concentrations of electrolyte components are determined externally using a separate monitoring system, which reports them to the controller. In other embodiments raw information collected from the system is communicated to the controller which conducts concentration determinations from the raw data. In both cases the controller is configured to adjust dosing parameters in response to these signals and/or concentrations such as to maintain homeostasis in the system. Further, in some embodiments, volume sensors, fluid level sensors, and pressure sensors may be employed to provide feedback to the controller.
(54) As mentioned, in some embodiments the anode chamber is coupled to a pressure regulator (e.g., pressure regulator 160), which is capable of equalizing the pressure in the anode chamber with atmospheric pressure. Such pressure-regulating mechanism is described in detail in U.S. application Ser. No. 13/051,822 titled ELECTROLYTE LOOP FOR PRESSURE REGULATION FOR SEPARATED ANODE CHAMBER OF ELECTROPLATING SYSTEM filed on Mar. 18, 2011 and naming Rash et al. as inventors, which is incorporated herein by reference in its entirety.
(55) The apparatus and processes described hereinabove may be used in conjunction with lithographic patterning tools or processes, for example, for the fabrication or manufacture of semiconductor devices. Typically, though not necessarily, such tools/processes will be used or conducted together in a common fabrication facility. Lithographic patterning of a film typically comprises some or all of the following steps, each step enabled with a number of possible tools: (1) application of photoresist on a workpiece, i.e., substrate, using a spin-on or spray-on tool; (2) curing of photoresist using a hot plate or furnace or UV curing tool; (3) exposing the photoresist to visible or UV or x-ray light through a mask using a tool such as a wafer stepper; (4) developing the resist so as to selectively remove resist and thereby pattern it using a tool such as a wet bench; (5) transferring the resist pattern into an underlying film or workpiece by using a dry or plasma-assisted etching tool; and (6) removing the resist using a tool such as an RF or microwave plasma resist stripper. This process may provide a pattern of features such as Damascene, TSV, RDL, or WLP features that may be electrofilled with silver tin using the above-described apparatus. In some embodiments, electroplating occurs after the resist has been patterned but before the resist is removed (through resist plating).
(56) As indicated above, various embodiments include a system controller having instructions for controlling process operations in accordance with the present invention. For example, a pump control may be directed by an algorithm making use of signals from the level sensor(s) in the pressure regulating device. For example, if a signal from a sensor indicates that fluid is not present at the associated level, the controller may direct that additional make up solution or DI water be provided into the anolyte recirculation loop to ensure that there is sufficient fluid in the line that the pump will not operate dry (a condition which could damage the pump). Similarly, if the upper level sensor signals that fluid is present in the associated level, the controller may direct may take steps to reduce the amount of recirculating anolyte, as explained above, thereby ensuring that the filtered fluid in the pressure regulating device remains between the upper and lower levels of the sensors. Optionally, a controller may determine whether anolyte is flowing in the open recirculation loop using, for example, a pressure transducer or a flow meter in the line. The same or a different controller will control delivery of current to the substrate during electroplating. The same or a different controller will control dosing of make up solution and/or deionized water and/or additives to the catholyte and anolyte.
(57) The system controller will typically include one or more memory devices and one or more processors configured to execute the instructions so that the apparatus will perform a method in accordance with the present invention. Machine-readable media containing instructions for controlling process operations in accordance with the present invention may be coupled to the system controller.
Gettering Embodiments
(58) The disclosed embodiments concern hardware and processes suited for extracting a relatively dilute, more noble metal contaminant (e.g. silver), from an anode chamber containing a less noble metal anode (for example pure low alpha tin), which is termed gettering hardware and processes. In a particular embodiment, the getter removes unwanted Ag.sup.+ that finds its way into the SAC compartment and would otherwise react with the active Sn metal anode, eventually leading to various forms of incapacitation, including but not limited to: higher anode interfacial and cell plating voltages, particle formation, local or global anode passivation with use (charge) and over time. With the gettering processes and hardware, the anode is at least partially protected from passivation, and the risk from the various failure mechanisms outlined earlier is mitigated.
(59) Passivation affecting performance generally occurs after a considerable amount of Ag.sup.+ reacts on the tin anodes. Two different general classes of hardware and methods are disclosed herein: (1) a passive gettering approach and (2) an active gettering approach. The passive approach basically differs from the active approach with respect to method of noble metal removal from the anolyte. The passive approach relies on the removing noble metal ions from anolyte via a chemical removal (for example a metal-metal displacement reaction or a selective ion-exchange process). The active approach involves removal of the noble metal based on its more positive reduction potential and therefore by using primarily an electrochemically driven process.
(60) Regardless of whether passive or active gettering is employed, additional features may be provided in the separated anode chamber to promote uniform flow to, around and/or throughout (if porous) the cell anode or getter. In the case where there is slow transference between chambers, which may occur over long periods of time (e.g., several weeks), or due to a sudden inadvertent anode-to-catholyte electrolyte separation breach or backflow, uniform electrolyte flow to, around over or through the anode is usually desirable. Deposition of dissolved silver ion will occur at a greater propensity on portion of the anode where the supply of silver ion is greatest. This may be the portion where convective flow is greatest. Those higher flow portions of the anode will subsequently become progressively more extensively coated with a silver coating than other portions. As a result, those high-silver-film-covered portions of the anode will also be more resistive to tin dissolution. As a specific example, consider a peripheral (versus central) portion of the anode is exposed to a higher electrolyte flow. That region will have its tin surface more extensively coated with an un-reactive and dissolution-blocking silver film. Conversely, the center regions of the anode will have relatively less silver coating, and have a smaller amount of the local surface blocked by the silver film. Further, if the anode is a porous anode, the lowest section of the anode is largely un-reactive to the electrolytic dissolution process until layers of materials (e.g., particles, nuggets, or spheres) are electro-anodized first. Therefore, these lower anode portions continue to accumulate any silver ions from the anolyte, integrated over a long period of time (several weeks to even several months).
(61) When the particular layer of tin active anode is finally exposed due to the reaction/dissolution of upper layers above them, and when they are then called upon to deliver tin and current to plate a wafer, more current will tend to emanate (originate) from the region where there is less silver surface coating. In this example, the central region, having a relatively lower flow, will have accumulated less silver coating (e.g. 50%), vs. the edge (e.g. 80%). Unfortunately, to provide radially uniform deposition on the work piece, the average local anode current density should be uniform with radius. However, the microscopic effective local current density (measured as the average local current density divided by the fraction of non-silver coated portion of the electrode) must be significantly greater in the high-silver-coverage portion of the anode in order to maintain the required radial uniform average local anode current density. Because the anode metal phase is generally held at nearly the same potential throughout, and regions of higher silver coverage have higher anodic dissolution kinetic resistance, those regions will have a lower average local anode current density. That local average local anode current density can lead to a non-favorable shift in the globally non-uniform current distribution on the wafer (make it progressively more non-uniform as the % difference in radial silver content increases with anode depth during use). To avoid such a situation, having the fraction of non-silver coated portion radially uniform by supplying uniform flow to, around and through the anode, enables one to maintain radially uniform within wafer uniformity (WIW).
(62) A manifold for delivering anolyte to the anode may provide substantially uniform distribution over the anode surface in the radial and azimuthal directions.
(63) As shown in
(64) Passive Gettering
(65) In passive gettering, a suitable material is used to remove or reduce unwanted contamination by reactive noble ions (e.g., Ag.sup.+ ions). In certain embodiments, passive gettering is used to remove traces of such noble ions from a SAC compartment. As mentioned, a passive gettering approach relies on a chemical mechanism and therefore need not integrate the gettering material in an electrode of an electrochemical cell. Typically, a passive gettering material is placed in the path of anolyte flowing, at least partially, toward the anode in the SAC compartment. Certain suitable locations for the gettering material are presented in the embodiments discussed below. See for example the embodiments depicted in
(66) In various embodiments, the gettering material is solid and does not at any time introduce foreign or incompatible specie(s) into the anolyte which would interfere with the plating reaction. For example, a metal, M, that is much less noble than silver, is capable of gettering Ag.sup.+ by the following general reaction: M(s)+nAg.sup.+.fwdarw.nAg(s)+M.sup.n+. However, this metal ion, M.sup.n+, is introduced in the electrolyte. Hence, one suitable gettering material for SnAg system is solid (low alpha) tin, which produces low alpha Sn.sup.2+ ions as the byproduct of the gettering process, a component of the electrolyte. So, in this example, the metal of the passive getter is the same as the active anode itself.
(67) In another example of a passive-type metal displacement type gettering process, the gettering material is a metal different than that of the active anode. One may employ a getter metal whose reduction potential is sufficiently more negative (less noble) than either of the metals of the alloy to be plated. As a particular example, a suitable metal for plating tin-silver solders should be less noble and have a standard reduction potential more negative than both silver (E=+0.799V vs. NHE) and tin (E=0.123 vs. NHE). The material also should not corrode aggressively in the anolyte (e.g. if using an acidic electrolyte, the material should not spontaneously and rapidly dissolve via a coupled corrosion reactions of the electrolyte to form hydrogen). Depending on particularly solutions pH, anion, and other factors, exemplary non-tin suitable SnAg getter materials include nickel (E=0.23V vs. NHE), cobalt (E=0.28V vs. NHE), and indium (E=0.338V vs. NHE).
(68) In a third example of a passive-type gettering process, the gettering material is an insoluble inorganic compound (of the anode metal material in some cases, e.g. Sn when plating SnAg) which is (1) substantially insoluble in the anolyte, (2) will react with silver ions, and (3) forms an insoluble inorganic silver compound. As a particular example of this type of getter material, tin (II) sulfide, whose solubility is estimated to be 0.000002 g/L may react to form silver (I) sulfide, having a solubility estimated to be 910.sup..sup.4 g/L.
(69) In yet another example of a passive-type gettering process, the gettering material is an ion-selective ion-exchange-resin, selective for removal of the more noble metal ion. Ion-exchange resins containing mercapto-, sulfide and thiol terminated end groups bound to a polymeric matrix background would be suitable.
(70) In certain embodiments where the passive metal getter material is the same species as the anode (e.g. a low alpha tin getter and a low alpha tin anode), the sacrificial getter metal (tin) is not physically touching, electrically connected to, or otherwise in chemical communication with the anode, except through ionic connection via the electrolyte; the getter material is exposed to the electrolyte that is exposed to the anode. The getter metal of the getter apparatus is not an anode and is not used as an anode at any time, even though the two may be located in the same chamber, or exposed to the same electrolyte. The two elements (anode and passive getter) in the system and do not function the same. They are differentiated in that the passive getter it is not connected to the plating electrical circuit and its electrical potential is allowed to float at the local electrochemical potential in the solution at the physical position in the system. That potential at the getter surface relative to the anode may be modulated by the applied current through the cell, though there is no external circuit for any current to pass into or out of the passive getter.
(71) The gettering process example, Sn.sub.getter(s)+2Ag.sup.+.fwdarw.Sn.sup.2++2Ag(s), is the same chemical reaction that would otherwise occur with the active Sn anode, leading to passivation, but the role of the getter is to have that process preferentially occur on the getter electrode. To that end, design variables for the getter assembly include the location of the getter (placement within the cell and relative to the anode and within the SAC system), flow distribution within and/or around the getter, and the getter's physical shape, form factor, total mass and composite particle size, and several other factors influencing the available interfacial surface area.
(72) In some implementations, the physical form for the getter is one whose surface area is greater than that of the anode, for example about 2 times or more greater, or about 10 times or more greater, than the anode. To achieve this, getters (passive or active) may be designed to maximize the surface-area-to-volume of the getter material. This may be accomplished by, for example, providing the getter material in the form of granules, large particles (e.g., about 100 um or larger diameter), small pellets, fine mesh or wires, and highly porous sintered metals. These same characteristics may be applied to active getter materials (e.g., silver) which are described below. A very large effective surface area maximizes the gettering chemical or electrochemical reaction rate and success of complete or near complete gettering within minimal fluidic passes and before reacting with the anode.
(73) In one embodiment, as depicted in
(74) In another embodiment, the getter is situated within the SAC compartment 205 and is placed below the tin anode 203. This configuration is illustrated in
(75) The anode to getter spacer material can be made to be porous, perforated or with flow exit paths around the perimeter, to allow flow exit path to the remaining SAC compartment above. Alternatively, if the anode is monolithic and/or if flow though the anode is not required, the spacer and electronically isolating material may be a sheet of dielectric material. These embodiment and approaches have the advantage of utilizing the significantly larger volume in the SAC cell to maximize the gettering process by virtue of larger volume.
(76) As one particular exception to the above, one embodiment provides an apparatus similar to
(77) Another embodiment is depicted in
(78) It is possible that when the cell is operating or plating, an indirect corrosion phenomena of the getter material may occur. If there is an electric field in the cell such that the lower section of the getter is at a more anodic (positive potential) than the upper half, this in the long term can result in the lower section of the getter slowly dissolving out Sn.sup.2+, and the upper section re-plating tin on it. To minimize this impact, one approach is to make the getter thin, and in some embodiments be composed of a multiple thin laminates of electrically isolated layers, each having a porous membrane separating it from the next sections. In this manner, there is no net consumption or generation of the getter by corrosion, and a favorable process of self-regeneration of new tin surface, available for silver gettering, can occur, extending the life of the getter.
(79)
(80) As shown in
(81) As shown in
(82) Active Gettering
(83) In the active gettering concept, an electrolytic process for removal of noble metal ions is driven by (1) an auxiliary low voltage power supply connecting the getter electrode to the anode with the getter polarized at, or slightly positive of (e.g. 50-400 mV positive) the anode potential, or (2) electrically connecting the getter element to the anode, either directly, or through a current controlling resistor. It should be understood that the counter electrode of the gettering electrode need not be the anode of the plating cell. In some embodiments, described more fully below and particularly with reference to
(84) In active gettering, a suitable material is used as an electrode to electrochemically remove unwanted contamination by reactive noble ions (e.g., Ag.sup.+ ions) from the SAC compartment. An active gettering electrode is placed in the path of anolyte flowing, at least partially, toward the anode in the SAC compartment. In certain embodiments, the gettering electrode is provided in a separate chamber or compartment located outside the principal SAC region. See for example the schematic illustration of
(85) Typically, the getter material is present in a quantity sufficient to remove the amount of noble metal ions conservatively expected to enter the SAC over an extended time period, e.g., at least about a day or at least about two days or at least about a week. Of course, these periods can vary depending on the throughput of the system and other factors. Typically, the active getter electrode has a surface area sufficient to remove a large fraction of the noble metal ions in the anolyte flowing through it. For example, the getter electrode may be designed to remove at least about 90% of noble ions flowing through it, or at least about 95% of such ions, or at least about 99% of such ions, or at least about 99.9% of such ions. The gettering electrode material may be relatively inert to the anolyte. Examples of suitable materials are presented elsewhere herein.
(86) In active gettering, the cathode getter may include a high surface area working cathode electrode. The electrode can be located within the anode chamber (e.g. below the anode). Alternatively, as illustrated in
(87) In a direct getter electrode connection method, a power supply is not used. Rather, the deposition of noble ions occurs by separating the spontaneous displacement reduction and oxidation processes to occur at two different locations. Silver deposition occurs at the getter electrode and tin dissolution occurs at the plating cell anode, which is electrically connected to the getter. The preference for the reaction to occur on the getter is driven by the higher surface area and, possibly, the lower kinetic resistance for plating on the purer metal of the getter (e.g. the presence of tin, from the anode, may kinetically impede or poison the rate at which silver ion reduction will occur on that surface, due to the formation of a heavy metal silver-metal alloy). Therefore, silver can be removed on a high surface area silver getter, and can drive tin metal ion dissolution for the anode. The potential for silver reduction will vary with silver concentration and the presence of silver complexer in the SAC compartment, but typically will be positive of tin reduction. So, rather than the tin corroding and electrons flowing though the anode to another location to complete the circuit and enable silver reduction, the electrons flow from the anode though an external lead spontaneously to the getter electrode, to reduce the silver there instead.
Sn.fwdarw.Sn.sup.+2+2e(E0.13V)Anode:
Ag.sup.++e.fwdarw.Ag(E+0.8 to +0.4V vs. NHE)Getter:
Ag.sup.++Sn.fwdarw.Sn.sup.+2+Ag(Cell voltage 0.53 to 0.93V)Net:
(88) While the process can occur by simply shorting the anode and getter electrode (and even having the high surface area getter electrode in physical contact directly with the anode), in certain embodiments, the electrode getter is provided in a separate, easily removable and changeable element such as a cartridge.
(89) The passage of current and charge between the anode and the getter is related to the amount (concentration) of noble metal, and a measure of the rate cumulated amount of silver removed. In certain embodiments, the current may be monitored to determine the concentration or change in concentration of the noble metal. In certain embodiments, the SAC is designed with (i) a separate housing for the getter allowing the anolyte to pass through the housing and return to the anode chamber, and (ii) an electrical connection between the electrochemical getter and the anode, which connection includes a calibrated resistor or similar device though which the current passing though the assembly can be monitored. Monitoring the current between the anode and the electrochemical getter allows one to detect catastrophic failure of the ion selective membrane, or some other source of leak, where a significant amount of silver enters the anode chamber. If left unchecked, a large concentration of silver in the anolyte can not only quickly passivate the anode, but it can also result in low silver plating on the wafer solder bumps, and a large change in plating uniformity. These conditions can dramatically lower the yield of high value wafers. Therefore, monitoring the current of the electrochemical getter of either the power supply regulated, or shorted configuration, may provide the added value of monitoring the life of the getter (time for replacement), and monitoring for cell catastrophic failure.
(90) As mentioned, an added benefit to active gettering is the ability to detect the presence of Ag.sup.+ contamination in the SAC. This can be accomplished without the addition of significant additional equipment/components or setup. In the absence of Ag.sup.+ contamination, there will be a low level of electrical current generated from the active gettering electrode, primarily driven by the reduction of oxygen when the getter potential is above 0V NHE. As oxygen is reduced by the process, the current will decrease to a steady low value associated with the rate of oxygen uptake in the SAC. The process has been shown to be largely able to be stopped completely by keeping a nitrogen gas layer above the exposed portions of the SAC electrolyte. Depending on the source of the Ag.sup.+ contamination, upon gettering, a peak or a sustained elevated current will flow through the electrical circuit. Thus, monitoring the current in this circuit will provide a direct indication of the presence of Ag.sup.+ in the system and the gettering process.
(91) Further, the reduction of dissolved atmospheric oxygen at the getter cathode provides an additional benefit. Low alpha tin electrolyte is expensive, and anything that can lower the operational cost will be of benefit. Using a tin active anode system lowers the cost and required use of low alpha tin electrolyte, but it generally cannot eliminate its use entirely. In addition to the strong inhibition of heavy metals like tin to water and proton reduction to form hydrogen, tin metal is reasonably stable in very strong acid despite its reduction potential being more negative than hydrogen formation. Also, because tin is a catalytically-poor oxygen reduction material, corrosion of tin by the reduction of oxygen is also largely inhibited. But the same statements are not true for silver or many other more noble metals. Therefore, the high surface area getter electrode can not only drive the reduction and removal of unwanted silver, but can also remove dissolved oxygen and drive the formation of hydrogen thereupon. Hence, the separation of the following cathodic and anodic processes between the catalytic getter electrode and the tin anode, allow for the spontaneous, and largely continuous, free formation of low alpha tin electrolyte from the low alpha tin anode.
(92) Ag Getter Cathodic Reactions
Ag.sup.+e.fwdarw.Ag (E+0.8 to +0.4V vs. NHE)
2H.sup.++2e.fwdarw.H.sub.2 (E0V vs. NHE)
O.sub.2 (dissolved)+4H.sup.++4e.fwdarw.2H.sub.2O (E+0.6V vs. NHE, 8 ppm O.sub.2)
(93) Sn Anode Anodic Reaction
Sn.fwdarw.Sn.sup.+2+2e(E0.13V)
(94) Suitable getter electrode materials include noble or semi noble metals, including but not limited to, silver, platinum, palladium, gold, iridium, osmium, ruthenium, osmium. Alternatively, less noble metal may be used to save cost. These may also be more easily manufactured into a high surface area form. In choosing these electrode materials, one should consider the requirement of avoiding corrosion of the base metal in the solution and that the material should be more noble than the anode metal, i.e., have a reduction potential positive of tin. One example is the use of copper screen, foam or mesh, particularly when its surface is coated and/or treated (e.g. by plating) with silver.
(95) Physical form factors leading to high surface area are preferred for similar reasons to the passive method: to help maximize the success of complete gettering or near complete gettering within minimal fluidic exposure and fluid passes. These physical form factors, include, but are not limited to, foils, granules, large particles, small pellets, fine mesh or wires, and highly porous sintered material.
(96) Similar to the passive gettering, the active gettering electrode can potentially be placed at various places in the SAC system. In a preferred embodiment, but not limited to, the gettering electrode is placed in a separate housing that is part of the SAC fluid recirculation, as depicted in
(97) In one embodiment the active gettering electrode can be constructed somewhat akin to a cartridge, allowing fairly easy replacements. In addition, the lifetime may be quite predictable by tracking the total amount of charge gettered by the gettering electrode. But to avoid internal corrosion of the getter under the influence of a gradient of potential within the anode chamber and cell, the getter should not generally be located or placed such that the extremities of the getter assembly are subjected to a substantial potential difference. Therefore, in one embodiment, the getter is housed between the anode and cathode and is substantially designed to be thin as possible and follow a surface of isopotential contours, similar to that shown in
(98) In the active getter embodiments described so far, the getter is electrically connected to the plating cell anode. In other words, the plating cell anode serves as the counter electrode to the getter working electrode or cathode. In other embodiments, a separate counter electrode is provided for the active getter cell. This separate electrode is an anode that is distinct from the plating cell anode. In some embodiments, the separate counter electrode is located relatively close to the getter electrode, at least in comparison to the location of the plate cell anode. The proximity and other features of the separate counter electrode may be chosen to promote current flow between it and the getter electrode, with relatively little current flowing between the getter electrode and the plating cell anode.
(99) In certain embodiments, the getter cell with separate anode is housed in its own chamber, separate from the SAC compartment. In one example, the getter cell chamber is implemented as a flow through assembly having both a silver extracting cathode and a local counter electrode which is also a source of low alpha tin (to prevent corrosion and enable the assembly to be shielded from field-induced corrosion). Certain implementations of a separate getter cell are depicted in
(100)
(101)
(102) Silver Ion and Leak Detection Probe
(103) In some embodiments, a silver ion presence and anode chamber leak detection probe are used (SILD probe). One embodiment of a silver ion leak detection probe 1301 is shown in
(104) The probe can be used to detect the amount of silver in a solution, or to warn of an unexpected high level of silver in the SAC compartment. The mode of operation in doing so can be varied, and just a few are mentioned here to clarity. In one mode of operating the leads of the device are connected to a power supply designed and suitable to maintain the potential between the two leads at a fixed potential. The potential between the leads may be held between approximately 0 V and 500 mV, with the silver detecting lead being held at the more positive potential. Current passing though the power supply and the SILD probe is then monitored by various common known means (e.g., and inductive or DC current meter, voltage across a resistance or a known value, etc.). In an alternative embodiment, the two leads of the SILD probe are connected together with a resistor of a known resistance, typically a quite low resistance that offer minimal resistance to the flow of current relative to the impedance of the device in the test solution. The impedance of the device depends on the size and surface areas of the electrodes of the SILD and the anolyte's conductivity, but typically a value of between about 10 ohm to 1 ohm will be suitable to measure a voltage across the resistance, and scale the current flowing between the SILD probes electrodes. The plating tool uses the SILD probe and monitors the voltage across the resistor or the current flowing though the SILD circuit, and is used to alert the operating system of a potential high level of silver in the anode chamber. With the cathode of the SILD held at a potential negative of the reduction potential of the silver (e.g. at or near tins reduction potential), any silver ion in the solution will be plated on the SILD cathode and the current can be measured. Anodic current is supplied to the SILD by the tin anode rod, generating stannic ions.
(105) It should be noted that the various embodiments presented herein are not mutually exclusive, and most if not all, can in fact be implemented simultaneously, thereby increasing overall effectiveness and robustness of the system in removing the unwanted Ag.sup.+ and hence protecting the tin anode of interest from passivation risk.
(106) It is to be understood that the configurations and/or approaches described herein are exemplary in nature, and that these specific embodiments or examples are not to be considered in a limiting sense, because numerous variations are possible. The specific designs and methods described herein may represent one or more of any number of design and processing strategies. As such, various acts and features illustrated may be implemented as shown, such as in the sequence illustrated, or in other sequences, in parallel, or in some cases omitted. Likewise, the order of the above described processes may be changed.
(107) The subject matter of the present disclosure includes all novel and nonobvious combinations and sub-combinations of the various processes, systems and configurations, and other features, functions, acts, and/or properties disclosed herein, as well as any and all equivalents thereof.