MANUFACTURING METHOD
20180009035 · 2018-01-11
Assignee
Inventors
- Mark Francis (Gloucestershire, GB)
- Richard Jordan (Gloucestershire, GB)
- Michael Barnes (Gloucestershire, GB)
Cpc classification
B22F2005/001
PERFORMING OPERATIONS; TRANSPORTING
B22F7/06
PERFORMING OPERATIONS; TRANSPORTING
B29C33/3842
PERFORMING OPERATIONS; TRANSPORTING
International classification
Abstract
A manufacturing method includes the steps of providing a mould containing a matrix material, providing an infiltrant material arranged so that, when molten, the infiltrant material will infiltrate into the matrix material, and heating the matrix material and the infiltrant material by induction heating using an induction heater. The induction heater includes a first coil and a second coil, wherein the first and second coils are energised independently of one another to allow increased control over the heating of different parts of the matrix material and infiltrant material within the mould.
Claims
1. A manufacturing method comprising the steps of: providing a mould containing a matrix material; providing an infiltrant material arranged so that, when molten, the infiltrant material will infiltrate into the matrix material; and heating the matrix material and the infiltrant material by induction heating using an induction heater; wherein the induction heater is operable to permit independent control over the heating of different parts of the matrix material and infiltrant material within the mould.
2. The method according to claim 1, wherein the induction heater includes at least a first coil and a second coil that are energised independently of one another to allow increased control over the heating of different parts of the matrix material and infiltrant material within the mould.
3. The method according to claim 2, wherein the energisation of the coils is such as to cause the matrix material to be heated to a temperature sufficient to maintain infiltration before melting of the infiltrant material occurs.
4. The method according to claim 2, further comprising, after the infiltrant material has infiltrated the matrix material, controlling the operation of the first and second coils to control cooling of the product.
5. The method according to claim 1, further comprising a step of using a cooling means to provide further control over the temperature of parts of the matrix material and infiltrant material within the mould.
6. The method according to claim 5, wherein the cooling means comprise a directional water cooling system operable to allow cooling of parts of the mould.
7. The method according to claim 1, further comprising using one or more temperature sensors located within the mould and operable to provide information to a control unit indicative of the temperatures within at least a part of the matrix material and infiltrant material, in controlling the induction heater.
8. The method according to claim 1, further comprising incorporating one or more metallic inserts or elements into at least one of the mould and the matrix material.
9. The method according to claim 1, further comprising an additional step of adjusting the position of the mould relative to the induction heater.
10. The method according to claim 1, wherein the infiltrant material is supplied, when molten, to a closed end of the mould.
11. The method according to claim 1, wherein the infiltrant material, prior to infiltration into the matrix material, is located remotely from the matrix material within the mould cavity.
12. The method according to claim 1, wherein during the infiltration process, the infiltrant material infiltrates upwardly through the matrix material and air displaced from the matrix material by the infiltrant material flows towards the surface of the matrix material.
13. The method according to claim 1 and employed in the manufacture of a drill bit.
14. The method according to claim 13, further comprising a step of locating a blank within the mould.
15. The method according to claim 14, wherein the temperature of an end part of the blank is maintained at a level sufficiently low that the material of the blank can be used to form a pin.
16. The method according to claim 15, wherein the blank is shaped to approximately the required pin shape prior to conducting the infiltration step, and subsequently, as part of the finishing operation, has threads formed thereon.
17. The method according to claim 1, wherein the heating step is undertaken with the mould located within an inert or reducing material atmosphere.
18. The method according to claim 1, wherein the mould is of an inductive material.
19. The method according to claim 18, wherein the mould is of graphite form.
20. The method according to claim 1, wherein the mould is of a non-inductive material.
21. The method according to claim 20, wherein the mould comprises a ceramic material shell.
22. A manufacturing method comprising the steps of: providing a mould containing a matrix material; providing an infiltrant material arranged so that, when molten, the infiltrant material will infiltrate into the matrix material, the infiltrant material being located within a reservoir remote from the matrix material.
23. The method according to claim 22, further comprising: heating the matrix material and the infiltrant material by induction heating using an induction heater including a first coil and a second coil; wherein the first and second coils are energised independently of one another to allow increased control over the heating of different parts of the matrix material and infiltrant material within the mould.
24. The method according to claim 22 and employed in the manufacture of a drill bit.
25. The method according to claim 22, further comprising a step of locating a blank within the mould.
26. The method according to claim 25, wherein the temperature of an end part of the blank is maintained at a level sufficiently low that the material of the blank can be used to form a pin.
27. The method according to claim 25, wherein the blank is shaped to approximately the required pin shape prior to conducting the infiltration step, and subsequently, as part of the finishing operation, has threads formed thereon.
28. A manufacturing method comprising the steps of: providing a mould containing a blank and a matrix material; providing an infiltrant material arranged so that, when molten, the infiltrant material will infiltrate into the matrix material; and heating the matrix material and the infiltrant material by induction heating; wherein during the heating step the blank an end part of the blank is maintained at a level sufficiently low that the material of the blank can be used to form a pin.
29. A drill bit manufactured according to the method of claim 1.
Description
[0025] The invention will further be described, by way of example, with reference to the accompanying drawings, in which:
[0026]
[0027]
[0028]
[0029] Referring firstly to
[0030] An upper part of the mould cavity 12 defines a funnel or reservoir region 18 within which is located an infiltrant material 20 in the form of nuggets of a suitable alloy material.
[0031] The provision of a mould 10 and method of filling the mould 10 to form an assembly of this form is substantially the same as would occur in a typical manufacturing method with the exception that, in the traditional manufacturing method the mould 10, once filled in this manner, would be placed within a conventional furnace for heating to achieve infiltration of the matrix material 16 by the infiltrant material 20.
[0032] In accordance with this embodiment of the invention, rather than place the mould 10 and its contents (the blank 14, matrix material 16 and infiltrant material 20) into a conventional furnace to achieve heating thereof, the filled mould 10 is instead heated using an induction heating apparatus 22. The induction heating apparatus 22 is arranged to permit increased control over the heating operation by allowing independent control over the heating of different parts of the filled mould 10 and its contents. In this embodiment, the induction heating apparatus 22 comprises a first induction heating coil 24 and a second induction heating coil 26. Each coil 24, 26 encircles a heating zone within which the mould 10 is positioned, in use. The coils 24, 26 are axially spaced apart from one another, and are controllable independently of one another to allow independent control over the heating and cooling of different parts of the matrix material and infiltrant located within the mould 10. As illustrated, the induction heating apparatus 22 further comprises a control unit 28 to which the coils 24, 26 are connected, the control unit 28 being operable to control the energisation of the coils 24, 26. Whilst a single control unit 28 is illustrated, it will be appreciated that its functions may be distributed amongst, for example, a plurality of control units provided in various locations.
[0033] As illustrated, a temperature sensor 30 in the form of a thermocouple arrangement extends into the mould 10 and is arranged to sense the temperature therein at a range of locations. The temperature information from the sensor 30 is supplied to the control unit 28.
[0034] In use, with the filled mould 10 located within the heating zone, the control unit 28 controls the energisation of the coils 24, 26 to control heating of the mould 10 and its contents. The output from the temperature sensor 30 is used by the control unit 28 in controlling the operation of the coils 24, 26 to achieve a desired temperature profile within the mould 10 and its contents.
[0035] By way of example, initially it may be desired to raise the temperature of the matrix material 16 within the layer 16a. This may be achieved by energisation of the second coil 26. Energisation of the second coil 26, by the application of an alternating current thereto, results in the generation of a magnetic field which is concentrated in the part of the heating zone within the coil 26. The varying magnetic field within the heating zone induces eddy currents within any inductive material objects or components located within the heating zone, and the electrical resistance of the inductive material objects, in combination with the induced eddy currents, causes the generation of heat within the inductive material objects which will dissipate by conduction and radiation to other locations within the mould 10, including to parts thereof of non-inductive material form. Accordingly, the energisation of the second coil 26 will result in heating of the lower part of the blank 14 which is of metallic form. Depending upon the nature of the matrix material, heat may also be generated therein. For example, if the matrix material includes metallic elements, or metallic coated elements, then the energisation of the second coil 26 be induce heat directly within the adjacent matrix material. Likewise, depending upon the material of the mould 10, or any coating applied thereto, heat may be generated therein through the energisation of the coil 26. By way of example, the mould 10 may be of graphite form and so be of an inductive material. Heat transfer between those parts of the mould 10 and the contents thereof in which heat is generated through the energisation of the coil 26 and those parts in which heat is not generated will result in heating of the entirety of the part of the assembly close to the coil 26, heating the matrix material 16.
[0036] After the temperature of the matrix material 16 has been raised to a desired level, for example around 1200° C., as sensed by the temperature sensor 30, the first coil 24 may be energised to heat the infiltrant material 20 and other parts of the assembly close thereto. Once the temperature of the infiltrant material 20 has been raised to a level sufficient to cause melting thereof, infiltration of the infiltrant material 20 into air spaces and other voids between the particles of the matrix material 16 will commence. The infiltrant material 20 will flow downward, substantially filling such spaces and voids, air being expelled therefrom towards the upper end of the mould, for example passing along a passage through which the temperature sensor 30 extends. By appropriate control over the energisation of the coils 24, 26, it can be ensured that the temperatures of the various parts of the mould and the contents thereof are held at a desired level to ensure complete infiltration thereof. The level of heat generated depends upon the magnitude of the applied current, and so by appropriate control over the applied currents, the operator has a good level of control over heating of the various parts of the mould and its contents. The level of heat generated can be changed very quickly, simply by adjusting the current applied to each coil.
[0037] After infiltration of the matrix material has been completed, the energisation levels of the coils 24, 26 can be controlled so as to allow the mould and its contents to cool in a controlled manner. By way of example, the energisation levels of the coils 24, 26 may be controlled in such a manner as to allow cooling of the materials located towards the bottom, closed end of the mould 10 prior to cooling of the materials closer to the open end of the mould 10, by maintaining the energisation of the first coil 24 at a higher level than that of the second coil 26. By controlling cooling in this fashion, the risk of damage to the moulded product through differential thermal contraction as the product cools, especially due to different levels of contract between the matrix material 16 and any infiltrant material 20 remaining within the reservoir 18, and between the matrix material 16 and the blank 14, can be reduced.
[0038] To assist in cooling, a water cooling arrangement 32 may be provided. As illustrated in
[0039] After cooling, the moulded drill bit component is removed from the mould and subjected to a number of finishing processes. These may include, for example, machining away of any infiltrant material 20 remaining within the reservoir 18 after completion of the moulding process. It may also involve machining away part of the matrix material to expose the end of the blank, and the welding of a pin component to the end of the blank, the pin component being used to allow the mounting of the drill bit to other parts of a drilling system, for example for use in boring holes in subsurface formations for the subsequent use in the extraction of hydrocarbons.
[0040] Conveniently, the steps of heating and cooling are undertaken with the mould 10 and its contents located within an inert or reducing material atmosphere, thereby avoid or reducing the likelihood of oxidation or the like of the materials within the mould 10.
[0041] The manufacture of products such as drill bits in this manner is advantageous in that the method permits faster, more accurate and repeatable heating of a mould and the contents thereof, resulting in a reduction in manufacturing variances. If required, temperature information from the sensor 30 may be stored, for example within the control unit 28, to provide a log indicative of the temperatures to which the various parts of the assembly have been exposed during the manufacturing process.
[0042] Whilst
[0043] In the arrangement of
[0044] In the arrangements of
[0045] Whilst in the arrangements described hereinbefore, a pair of coils 24, 26 is provided, it will be appreciated that more coils may be provided, if desired, providing a greater degree of control over the heating and cooling operations. If desired, the mould and its contents may be positioned in such a manner as to be movable relative to the coils, and/or the coils may be movable relative to one another, thereby permitting further control over the heating and cooling operations.
[0046] One or more of the coils may be located internally of the mould, for example within a sand core or mandrel 34 located within the blank 14. Furthermore, if desired, an internal cooling arrangement, for example located within the mandrel, may be provided to permit further control over the cooling operation.
[0047] As mentioned above, energisation of the coils results in the generation of heat within metallic components located within the mould and its contents. If desired, for example to aid in achieving a desired heating profile, one or more metallic inserts 38 (see
[0048] In the arrangements described hereinbefore, the method is employed in the manufacture of a drill bit comprising a matrix material body mounted upon a support. The invention is not restricted in this regard, and may be used in other applications. By way of example, the method of the invention may be employed in applying a relatively thin matrix material layer to the surface of a metallic material bit body, the matrix material layer serving to enhance the wear resistance of the bit body. In such an arrangement, as the matrix material layer is of relatively thin form, heating thereof may be achieved successfully relying upon heat transfer from the bit body which, being of metallic form, will be heated by the energisation of the coils. The mould may be of a non-inductive material, for example it could take the form of a relatively thin ceramic material shell.
[0049] Whilst specific embodiments of the invention are described hereinbefore, it will be appreciated that a wide range of modifications and alterations may be made thereto without departing from the scope of the invention as defined by the appended claims.