METHOD FOR MANUFACTURING PRESS MOLDED PRODUCT
20200206798 ยท 2020-07-02
Assignee
Inventors
- Kazuki SAKAMOTO (Kobe-shi, Hyogo, JP)
- Yasuhiro HAYASHIDA (Kobe-shi, Hyogo, JP)
- Kenichi WATANABE (Kobe-shi, Hyogo, JP)
- Takayuki KIMURA (Kobe-shi, Hyogo, JP)
Cpc classification
B21D53/88
PERFORMING OPERATIONS; TRANSPORTING
B21D22/06
PERFORMING OPERATIONS; TRANSPORTING
B21D22/24
PERFORMING OPERATIONS; TRANSPORTING
B62D25/04
PERFORMING OPERATIONS; TRANSPORTING
B21D24/00
PERFORMING OPERATIONS; TRANSPORTING
B21D35/006
PERFORMING OPERATIONS; TRANSPORTING
B21D22/26
PERFORMING OPERATIONS; TRANSPORTING
International classification
Abstract
A method for manufacturing a press molded product includes forming a plurality of corner portions in a pressed portion of a pressed member, providing the pressed member between a first die and a second die, and press molding the pressed portion to decrease a height of the pressed portion. The press molding includes forming a pair of first bent portions in the pressed portion by means of the corner portions, the pair of first bent portions being bent to protrude toward the second die, forming a second bent portion in the pressed portion by means of the corner portions while holding the pair of first bent portions by a pair of holding portions, the second bent portion being bent to protrude toward the first die from a position between the pair of first bent portions, and pressing and deforming the second bent portion.
Claims
1. A method for manufacturing a press molded product by press molding a pressed portion that has a bent shape and is formed in a pressed member having a plate shape, the method comprising: forming a plurality of corner portions in the pressed portion; providing the pressed member, having the corner portions formed in the pressed portion, between a first die and a second die; and press molding the pressed portion by relatively moving the first die and the second die toward each other to decrease a height of the pressed portion, wherein the press molding includes forming a pair of first bent portions in the pressed portion by means of the corner portions, the pair of first bent portion being bent to protrude toward the second die, forming a second bent portion in the pressed portion by means of the corner portions while holding the pair of first bent portions by a pair of holding portions that has a groove shape and is provided to be spaced apart from each other in the second die, the second bent portion being bent to protrude toward the first die from a position between the pair of first bent portions, and pressing and deforming the second bent portion.
2. The method according to claim 1, wherein in the press molding, the pressed portion is thickened.
3. The method according to claim 1, wherein in the press molding, the pressed portion is press molded so that the height of the pressed portion disappears after the molding
4. The method according to claim 1, wherein in the press molding, the pressed portion is press molded so that the pressed portion after being molded has a bent shape with a smaller height than the pressed portion before being molded.
5. The method according to claim 1, wherein in the press molding, peripheral portions of the pressed portion in the pressed member are clamped by the first die and the second die.
6. The method according to claim 1, wherein the pressed member is formed by hot pressing.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
[0026]
[0027]
[0028]
[0029]
[0030]
[0031]
[0032]
[0033]
[0034]
[0035]
[0036]
[0037]
[0038]
[0039]
[0040]
EMBODIMENTS OF THE INVENTION
[0041] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0042] [Press Molding Apparatus]
[0043]
[0044] The pressed member 30 is a plate material made of a metal material such as hard steel, mild steel, aluminum, titanium, or copper. The pressed member 30 includes the pressed portion 31 and peripheral portions 32 and 33 that are connected to each other to be in a single plate shape. The pressed portion 31 is a portion to be thickened as a result of the press molding. The peripheral portions 32 and 33 are connected to both ends of the pressed portion 31, and are bent to have an L-shaped cross section. The peripheral portions 32 and 33 are portions that are not pressed by the first die 10 and the second die 20.
[0045] As illustrated in
[0046] The pressed portion 31 before the pressing has a line length longer than the length along the undulations of an uneven area 91A, described later, in a press molded product 90 illustrated in
[0047] The pressed portion 31 is configured to have a bent shape as described above, so that a sufficient line length required for the thickening is ensured. More specifically, a longer line length can be ensured, compared with a comparative example illustrated in
[0048] As illustrated in
[0049] Furthermore, as illustrated in
[0050] The first-die center portion 11 and the first-die peripheral portions 12 are configured to be movable, in the vertical direction, by the drive unit 40 independently of each other. Specifically, only the first-die peripheral portions 12 can be moved up and down with the position of the first-die center portion 11 fixed, and only the first-die center portion 11 can be moved in the vertical direction with the positions of the first-die peripheral portions 12 fixed.
[0051] The first molding surface 11A of the first-die center portion 11 is provided with a pressing portion 14 having a shape protruding downward toward the second die 20. The pressing portion 14 is a center portion of the first molding surface 11A and protrudes downward beyond the portions on both sides thereof. As illustrated in
[0052] As illustrated in
[0053] The second-die center portion 21 includes a support portion 24 provided on a horizontal plane, and a molding portion 25 standing upward toward the first die 10, at substantially the center of the support portion 24. The lower press molding surface 20A is provided at the top of the molding portion 25. The lower press molding surface 20A is configured to include a continuous uneven area, as in the configuration of the upper press molding surface 10A, and has a length that is the same as the width of the uneven area 91A formed in the press molded product 90 illustrated in
[0054] As illustrated in
[0055] As illustrated in
[0056] In the second die 20, the second-die center portion 21 corresponds to a lower molding die portion that cooperates with the upper molding die portion 74 to press mold the pressed portion 31, and the second-die peripheral portions 22 correspond to lower clamping die portions that cooperate with the upper clamping die portions 75 and 76 to clamp and fix the peripheral portions 32 and 33. Thus, in this embodiment, the lower molding die portion and the lower clamping die portions are configured as separate portions.
[0057] The drive unit 40 is for lowering the first die 10 to approach the second die 20. Thus, the press space S can be reduced and the pressed portion 31 can be press molded. The drive unit 40 is disposed on the upper side of the first die 10 and has a hydraulic or electric piston capable of reciprocating movement. The first-die center portion 11 and the first-die peripheral portions 12 are pressed by this piston, and thus can be moved up and down independently of each other.
[0058] [Method for Manufacturing Press Molded Product]
[0059] Next, a process for press molding the pressed portion 31 using the press molding apparatus 1 will be described mainly with reference to a flowchart in
[0060] First, step S09 for preparing the pressed member 30 is performed. In step S09, first of all, a flat plate-shaped pressed member 30 made of various metal materials such as hard steel is prepared, and by processing this, a bent pressed portion 31 having the plurality of corner portions 31G is formed. Then, the pressed member 30 is softened by being heated in an electric furnace or by being energized and heated.
[0061] Next, step S10 for providing the pressed member 30 in the press molding apparatus 1 is performed. In step S10, the pressed member 30 softened by being heated is disposed between the first die 10 and the second die 20. In this process, as illustrated in
[0062] Next, step S20 for press molding the pressed portion 31 is performed. In step S20, the press space S is reduced by bringing the first die 10 closer to the second die 20, so that the pressed portion 31 is press molded to have the height H decreased. In step S20, bending step S21 illustrated in
[0063] First of all, in bending step S21, in the state illustrated in
[0064] By further lowering the first-die peripheral portions 12 in this state, the press space S is reduced, and the height H of the pressed portion 31 is gradually decreased. Then, when the height H of the pressed portion 31 decreases to or below a predetermined value, the pressed portion 31 is bent by means of the corner portions 31G, whereby the pair of first bent portions 31A that is bent to protrude toward the second die 20 and the second bent portion 31B that is bent to protrude toward the first die 10 from a position between the pair of first bent portions 31A are formed in the pressed portion 31 as illustrated in
[0065] Next, in deforming step S22, both the first-die center portion 11 and the first-die peripheral portions 12 are lowered by the drive unit 40, whereby the second bent portion 31B is pressed by the pressing portion 14 of the first die 10 while the first bent portions 31A are being held by the holding portions 20B as illustrated in
[0066] As described above, by press molding the pressed portion 31 in the height direction (that is, in the vertical direction) while preventing the material from flowing toward the peripheral portions 32 and 33, the pressed portion 31 is thickened in accordance with the decrease in the height H of the pressed portion 31. Thus, as illustrated in
[0067] [Press Molded Product]
[0068] Next, the press molded product 90 according to the present embodiment will be described with reference to
[0069] As illustrated in
[0070] [Operation and Effect]
[0071] Next, features as well as operations and effects of the press molding apparatus 1 and the method for manufacturing a press molded product according to the present embodiment will be described.
[0072] The press molding apparatus 1 is an apparatus that manufactures the press molded product 90 by press molding the bent pressed portion 31 having the plurality of corner portions 31G formed in the plate shaped pressed member 30. The press molding apparatus 1 has the first die 10 having the upper press molding surface 10A, the lower press molding surface 20A facing the upper press molding surface 10A so that the press space S in which the pressed portion 31 is accommodated is formed between the first die 10 and the second die 20, and the drive unit 40 that causes the first die 10 and the second die 20 to relatively move toward each other so that the press space S is reduced. The second die 20 is provided with the pair of concave groove shaped holding portions 20B that is provided while being spaced apart from each other and hold the two first bent portions 31A in the pressed portion 31. The first die 10 includes the pressing portion 14 that is positioned between the two holding portions 20B, has a shape protruding toward the second die 20, and presses the second bent portion 31B in the pressed portion 31.
[0073] The method for manufacturing a press molded product is a method for manufacturing the press molded product 90 by press molding the bent shaped pressed portion 31 having the plurality of corner portions 31G formed in the plate shaped pressed member 30. This manufacturing method includes step S09 for preparing the pressed member 30, step S10 for providing the pressed member 30, with the corner portions 31G formed in the pressed portion 31, between the first die 10 and the second die 20, and step S20 for causing the first die 10 and the second die 20 to relatively move toward each other to decrease the height H of the pressed portion and press mold the pressed portion 31.
[0074] In step S09 for preparing the pressed member 30, the flat plate-shaped pressed member 30 is prepared and processed so that the bent pressed portion 31 having the plurality of corner portions 31G is formed. Then, the pressed member 30 is softened by being heated in an electric furnace or by being energized and heated.
[0075] In step S10 in which the pressed member 30 is provided between the first die 10 and the second die 20, the pressed member 30, with the bent pressed portion 31 having the plurality of corner portions 31G, prepared in step S09 is provided between the first die 10 and the second die 20.
[0076] In step S20 in which the press molding is performed, the pair of first bent portions 31A that is bent to protrude toward the second die 20 is formed in the pressed portion 31 by means of the corner portions 31G. Then, the second bent portion 31B that is bent to protrude toward the first die 10 from the position between the pair of first bend portions 31A is formed in the pressed portion 31 by means of the corner portions 31G, while the pair of first bent portions 31A is being held by the pair of holding portions 20B that has a groove shape and is provided to be spaced apart from each other in the second die 20. Then, the second bent portion 31B is pressed by the pressing portion 14 of the first die 10 to be deformed, so that the pressed portion 31 is thickened.
[0077] With the above feature, the pressed portion 31 is formed in a bent shape with the line length required for thickening ensured. By press molding the pressed portion 31 to decrease the height H, the thickened portion can be formed. Therefore, compared with the comparative example illustrated in
[0078] In the method for manufacturing a press molded product described above, the first bent portions 31A and the second bent portion 31B are formed in the pressed portion 31 in press molding step S20. More specifically, press molding step S20 includes bending step S21 and deforming step S22. In bending step S21, the first bent portions 31A and the second bent portion 31B are formed in the pressed portion 31 by means of the corner portions 31G. In deforming step S22, the second bent portion 31B is pressed and deformed while the first bent portions 31A are being held by the holding portions 20B. With the first and second bent portions 31A and 31B thus formed in the pressed portion 31 by means of the corner portions 31G during the press molding, the material flow is facilitated so that the first and second bent portions 31A and 31B can be easily formed at desired positions, whereby the press molded product with a desired shape can be more appropriately obtained. The first and second bent portions 31A and 31B need not to be formed in advance before press molding, and thus a more efficient manufacturing process can be achieved.
[0079] In press molding step S20 in the method for manufacturing a press molded product, the pressed portion 31 is press molded to have a larger thickness than the portion other than the pressed portion 31 (the peripheral portions 32 and 33) in the pressed member 30. Thus, the press molded product 90 having a partially thickened portion to have improved strength can be manufactured.
[0080] In press molding step S20 in the method for manufacturing a press molded product, the pressed portion 31 is press molded so that the height H of the pressed portion 31 disappears after the molding, that is, until the positions of the end portions of the peripheral portions 32 and 33 connected to the pressed portion 31 coincides with that of the pressed portion 31 in the vertical direction. As a result, the thickened amount of the pressed portion 31 can be more increased, whereby the press molded product 90 with more improved strength can be manufactured.
[0081] In the method for manufacturing a press molded product, the pressed member 30 has the peripheral portions 32 and 33 connected to the end portions of the pressed portion 31. In press molding step S20, the portions of the peripheral portions 32 and 33 connected to the pressed portion 31 are clamped by the first die 10 (first-die peripheral portions 12) and the second die 20 (second-die peripheral portions 22). Thus, the flow of the material from the end portions of the pressed portion 31 toward the center portion during the press molding can be facilitated, whereby uneven distribution with an excessive amount of material being in the end portions of the pressed portion 31 can be more effectively suppressed.
[0082] In the method for manufacturing a press molded product, the first die 10 includes the first-die center portion 11 having the pressing portion 14 and the first-die peripheral portions 12 that are formed separately from the first-die center portion 11 and are configured to be movable independently from the first-die center portion 11. In press molding step S20, the first bent portions 31A and the second bent portion 31B are formed in the pressed portion 31 by means of the corner portions 31G by moving the first-die peripheral portions 12, and then the second bent portion 31B is pressed by the pressing portion 14 to be deformed. More specifically, in bending step S21, the first bent portions 31A and the second bent portion 31B are formed in the pressed portion 31 by means of the corner portions 31G by moving the first-die peripheral portions 12 downward. In deforming step S22, the second bent portion 31B is pressed by the pressing portion 14 to be deformed by moving the first-die center portion 11 downward. Thus, the movement of the first-die center portion 11 can start after the second bent portion 31B is formed in the pressed portion 31 during the press molding, whereby the second bent portion 31B can be more reliably pressed by the pressing portion 14.
[0083] In the method for manufacturing a press molded product, the distance L1 between the pressing portion 14 and the second die 20 is the same as the distance L2 between the holding portion 20B and the first die 10, at the timing when press molding step S20 is completed. Thus, the pressed portion 31 can have a uniform thickness.
[0084] In press molding step S20 in the method for manufacturing a press molded product, the pressed portion 31 is provided with the uneven area 91A. Accordingly, the press molded product 90 that is reinforced by the uneven area 91A to have improved strength can be manufactured.
[0085] In the method for manufacturing a press molded product, the pressed member 30 is formed by hot pressing. As described above, in the present embodiment, the flow of the material in the pressed portion 31 can be controlled during press molding, whereby a desired thickened amount can be obtained even when hot pressing facilitating the material flow is performed.
Another Embodiment
[0086] In the above-described method for manufacturing a press molded product, the pressing portion 14 is provided in the first die 10. Alternatively, the pressing portion may be provided in the second die 20.
[0087]
[0088] As illustrated in
[0089] The second-die center portion 21 includes the support portion 24 provided on a horizontal plane, the molding portion 25 standing upward toward the first die 10, at substantially the center of the support portion 24, and a molding center portion 28 arranged at the center of the molding portion 25. The molding center portion 28 is configured to be movable, by a drive unit 41, in the vertical direction.
[0090] The pressing portion 29 having a shape recessed downward toward the first die 10 is provided on a mold surface 28A of the molding center portion 28. The pressing portion 29 is a center portion of the mold surface 28A and is recessed downward beyond the portions on both sides thereof. As illustrated in
[0091] Next, step S20 (
[0092] First of all, in bending step S21, in the state illustrated in
[0093] Then, as illustrated in
[0094] Next, in deforming step S22, the first die 10 is lowered by the drive unit 40, and the molding center portion 28 of the second die 20 is lowered by the drive unit 41 (here, the lowered amount of the molding center portion 28 is smaller than the lowered amount of the first die 10). The second bent portion 31B is pressed by the first die 10 and the pressing portion 29 of the molding center portion 28 of the second die 20, while the first bent portions 31A are being held by the holding portions 20B as illustrated in
[0095] As described above, by press molding the pressed portion 31 in the height direction (that is, in the vertical direction) while preventing the material from flowing toward the peripheral portions 32 and 33, the pressed portion 31 is thickened in accordance with the decrease in the height H of the pressed portion 31. Thus, the pressed portion 31 has a thickness larger than thicknesses of the peripheral portions 32 and 33, whereby the press molded product that is partially thickened is manufactured. Furthermore, the pressed portion 31 after molding is not only thickened, but also has the uneven area having a shape conforming to the uneven surfaces of the upper and lower press molding surfaces 10A and 20A. When the press molding is thus completed, the first die 10 is raised by the drive unit 40, and then the press molded product is taken out.
[0096] In the other embodiment, the pressed portion 31 is formed in a bent shape with the line length required for thickening ensured. By press molding the pressed portion 31 to decrease the height H, the thickened portion can be formed. Therefore, compared with the comparative example illustrated in
[0097] In press molding step S20 in the method for manufacturing a press molded product according to the other embodiment described above, the first bent portions 31A and the second bent portion 31B are formed in the pressed portion 31 by means of the corner portions 31G by moving the first die 10, and then the second bent portion 31B is pressed by the pressing portion 29 of the second die 20 to be deformed. More specifically, in bending step S21, the first bent portions 31A and the second bent portion 31B are formed in the pressed portion 31 by means of the corner portions 31G by moving the first die 10 downward and moving the molding center portion 28 of the second die 20 upward. In deforming step S22, the second bent portion 31B is pressed by the pressing portion 29 to be deformed by moving the first die 10 downward. Thus, the second bent portion 31B can be more easily formed by the pressing portion 29, and the second bent portion 31B can be more reliably pressed.
[0098] It should be understood that the embodiments disclosed herein are illustrative and non-restrictive. The scope of the present invention is defined by the scope of claims and not by the description above. The scope of the present invention is intended to include meaning equivalent to the terms of the claims as well as any modifications within the scope of claims.
DESCRIPTION OF REFERENCE NUMERALS
[0099] 1: Press molding apparatus [0100] 10: First die [0101] 10A: Upper press molding surface [0102] 14: Pressing portion [0103] 20: Second die [0104] 20A: Lower press molding surface [0105] 20B: Holding portion [0106] 29: Pressing portion [0107] 30: Pressed member [0108] 31: Pressed portion [0109] 31A: First bent portion [0110] 31B: Second bent portion [0111] 31G: Corner portion [0112] 31L: Linear portion [0113] 32: Peripheral portion [0114] 33: Peripheral portion [0115] 40: Drive unit [0116] 90: Press molded product [0117] 91: Top plate portion [0118] 91A: Uneven area [0119] P1: Connection portion [0120] P2: Connection portion [0121] S: Press space [0122] T1: Thickness [0123] T2: Thickness