METHOD OF MAKING FIRE RETARDANT MATERIALS AND RELATED PRODUCTS

20240191430 ยท 2024-06-13

Assignee

Inventors

Cpc classification

International classification

Abstract

Methods for making fire retardant material including fire retardant cellulosic insulation are described. The methods include arrangements for partitioning fibers derived from fiber feedstocks and adding at least a portion of fibers of one or more feedstocks and a fire retardancy chemical compound to a mixer prior to fiber drying. The fibers may be disentangled and/or partitioned prior to mixing with the fire retardancy chemical compound. The fibers may be partially dewatered prior to the drying or other steps of the methods. The feedstock may include old newsprint (ONP), old corrugated containers (OCC), and/or other cellulose-based materials. The method further includes retaining the fibers feedstock and the chemical compound together for enough time to ensure adherence and impregnation of enough of the chemical to and in the fibers after the drying process. Fibers may be partitioned and disentangled prior to, during, and/or after treatment with the fire retardancy compound. The fire retardant cellulose insulation may be a standalone product or may be a component of a finished insulation end product.

Claims

1. A method for making a fire-retardant cellulose insulation comprising the steps of: partitioning a primary stream of fibers that contains short and long fibers into a first stream and a second stream, wherein the fraction of the fibers of the first stream that are short fibers is higher than the fraction of short fibers in the primary stream and the fraction of the fibers in the seconds stream that are long fibers is higher than the fraction of long fibers in the primary stream; introducing the fibers of the second stream to a processing system for making a product other than the fire-retardant insulation, partially dewatering fibers of the first stream; introducing the fibers of the first stream to a mixer; introducing one or more solvents to the mixer; introducing one or more fire-retardant chemicals to the mixer; mixing the fibers, the one or more solvents and the one or more fire-retardant chemicals in the mixer long enough to retain the one or more fire-retardant chemicals on and within the fibers of the first stream to form treated fibers; and drying the treated fibers to form the fire-retardant cellulose insulation.

2. The method of claim 1 further comprising the step of combining the fire-retardant cellulose insulation with one or more other components to make a finished insulation product.

3. The method of claim 1 further comprising the step of disentangling, in a moist state, the fibers of the first stream after the step of partitioning the fibers and before completing the drying of the treated fibers.

4. The method of claim 1 wherein the feedstock includes one or more recycled material feedstocks.

5. The method of claim 1 further comprising the step of adding one or more additives to the mixer before or during the mixing step.

6. The method of claim 1 further comprising the step of disentangling, in a moist state, the fibers of the first stream after the step of partitioning the fibers, and then subsequently partitioning the fibers again before the drying of the treated fibers is completed.

7. The method of claim 1 further comprising the step of disentangling, in a moist state, the fibers of the first stream after the step of partitioning the fibers, and then subsequently disentangling the fibers again before the drying of the treated fibers is completed.

8. The method of claim 1 further comprising the step of disentangling the treated fibers after the step of drying.

9. The method of claim 1 further comprising the step of classifying the treated fibers after the step of drying.

10. The method of claim 1 further comprising the step of recovering dust generated in the production process by adding recovered dust to the mixer.

11. The method of claim 1 further comprising the step of recovering residual fiber dust from the treated fibers after the step of drying.

12. The method of claim 11 wherein the step of recovering residual fiber dust from the treated fibers utilizes a dry classifier to partition the residual fiber dust from the treated fibers.

13. The method of claim 12 further comprising the step of combining portions of residual fiber dust together with fibers to form treated fiber superstructures.

14. The method of claim 13 wherein the step of combining portions of residual fiber dust together includes combining the portions of residual fibers and dust together with a binder.

15. The method of claim 13 further comprising the step of returning the treated fiber superstructures to the mixer.

16. The method of claim 1 wherein the step of partitioning the fibers of the one or more feedstocks includes partitioning the fibers using a screening system while the fibers are in a slurry with a consistency below 10%.

17. The method of claim 1 wherein the step of partitioning the fibers of the one or more feedstocks includes partitioning the fibers using a cyclonic separation system while the fibers are in a slurry with a consistency below 10%.

18. The method of claim 1 wherein the step of partitioning the fibers of the one or more feedstocks includes partitioning the fibers after a pulping process is used to disentangle the fibers.

19. The method of claim 1 wherein the one or more feedstocks includes one or more of cereal straw, animal feathers, and other lignocellulosic agricultural byproducts.

20. A method for making a fire-retardant cellulose insulation comprising the steps of: disentangling fibers of one or more feedstocks while in at least a partially moist state; introducing fibers of the one or more feedstocks to a mixer; introducing one or more solvents to the mixer; introducing one or more fire-retardant chemicals to the mixer; mixing the fibers, the one or more solvents and the one or more fire-retardant chemicals in the mixer long enough to retain the one or more fire-retardant chemicals on and within the fibers to form treated fibers; and drying the treated fibers to form the fire-retardant cellulose insulation.

21. The method of claim 20 further comprising the step of combining the fire-retardant cellulose insulation with one or more other components to make a finished insulation product.

22. The method of claim 20, wherein at least a portion of the disentanglement of the fibers takes place prior to the mixing process.

23. The method of claim 20 wherein at least a portion of the disentanglement of the fibers takes place within the mixer.

24. The method of claim 20 wherein at least a portion of the disentanglement of the fibers takes place during the drying process and before the material is fully dried.

25. The method of claim 20 wherein the fiber stream is partitioned after disentanglement of the fibers, and prior to when the fiber stream is fully dried.

26. The method of claim 20 wherein the feedstock includes one or more recycled material feedstocks.

27. The method of claim 20 further comprising the step of adding one or more additives to the mixer before or during the mixing step.

28. The method of claim 20 further comprising the step of partitioning the treated fibers after the step of drying.

29. The method of claim 20 further comprising the step of recovering residual fiber dust from the processing of fibers by adding the dust to the mixer.

30. The method of claim 20 further comprising the step of recovering residual fiber dust from the treated fibers after the step of drying.

31. The method of claim 30 wherein the step of recovering residual fiber dust from the treated fibers comprises directing the treated fibers to a dry classifier.

32. The method of claim 30 further comprising the step of combining portions of residual fiber dust together with dust to form treated fiber superstructures.

33. The method of claim 32 wherein the step of combining portions of residual fiber dust together includes combining the residual fiber dust with a binder.

34. The method of claim 32 further comprising the step of returning the treated fiber superstructures to the mixer.

35. The method of claim 20 further comprising the step of partitioning the fibers, wherein the step of partitioning the fibers of the one or more feedstocks includes screening the fibers while in a slurry state with a consistency below 10%.

36. The method of claim 20 further comprising the step of partitioning the fibers, wherein the step of partitioning the fibers of the one or more feedstocks comprises using cyclonic separation of streams while in a slurry state with a consistency below 10%.

37. The method of claim 20 wherein the one or more feedstocks includes one or more of cereal straw, animal feathers, and other lignocellulosic agricultural byproducts.

38. The method of claim 20 further comprising the step of at least partially dewatering the partitioned fibers prior to the step of introducing the partitioned fibers to the mixer.

Description

BRIEF DESCRIPTION OF THE DRAWING

[0031] The FIG. 1s a simplified block diagram representation of the method stages and primary system components associated with the manufacture of the cellulose insulation of the present invention. Dashed lines represent optional features, components and steps.

DETAILED DESCRIPTION OF EMBODIMENTS OF THE INVENTION

[0032] While the following description is directed to the embodiment of the invention wherein an organic cellulosic insulation is made, it is to be understood that the invention is not limited thereto. Instead, the present invention provides methods to produce cellulose-based insulation having adequate fire retardancy using one or more recycled cellulose-based feedstock material in a cost-effective way. Additionally, the present invention provides for the fabrication of such a product while reducing the inclusion of dust material in the finished product. The steps of the method as described may be done in different orders without deviating from the scope of the invention including, but not limited to, the order in which components are added to a mixer.

[0033] Referring generally to the FIGURE, a fire-retardant cellulose insulation of the present invention is created when cellulose-based feedstock material 10 that may include waste material referred to herein as recycled feedstock material, and/or other feedstock materials is/are combined with one or more fire retardancy chemical compounds to produce a fire-retardant cellulose insulation product. The fire-retardant cellulose insulation of the present invention may be a stand-alone insulation product or it may be combined with one or more other components having insulative and/or fire-retardance characteristics to form a multi-component insulation product. The one or more other components may be cellulose-based or they may be non-cellulose based. The one or more feedstock materials are reduced to fiber form prior to or in conjunction with combining with the one or more fire retardancy compounds in a liquid environment. The feedstock material 10, along with optional virgin feedstock 20 and/or recovered wet fibers 30 are transferred to a fiber generating apparatus such as a pulper 40, for example. Other means for generating fibers from the feedstock are known to those skilled in the art, and may also include recovering dry fiber streams from downstream processes.

[0034] The pulper 40 may be utilized for disentangling fibers or clumps of fibers from one another. The agitation of fibers in the presence of a liquid such as water can be an effective means of disentangling the fibers to an extent. Pulp generated in the pulper 40 may be transferred to a partitioning device 50 to remove contaminants and/or to classify fibers before introducing the fibers to a mixer 60. The partitioning device 50 may be a wet classification system, such as a screening system that intentionally divides fibers by fiber size. The partitioning device 50 may also be a cyclonic separator that intentionally divides heavy materials from lighter materials. The partitioning device 50 may also have multiple stages and multiple functions, such as combinations of cyclonic separators and screening systems, with the goal of partitioning fibers desired for one use from fibers desired for a different use and/or intentionally dividing out waste materials.

[0035] The fibers whether disentangled or partitioned, or any combination thereof, may be transferred to the mixer 60 or a portion, such as those that may be characterized as shorter fibers as defined herein, may be transferred to the mixer 60 while in an embodiment of the invention a remainder of the fibers are diverted to another process for making a product that is not the fire-retardant cellulose insulation, such as the fabrication of linerboard, container board, corrugated medium structures, combinations thereof, or other products, for example. The fibers directed to the mixer 60 for making the fire-retardant cellulose insulation are represented as a first stream of fibers as defined herein, and the remainder to be used for making other product are represented as a second stream of fibers as defined herein. The fibers of the first stream to be treated to become the insulation may be dewatered, at least partially, in dewatering apparatus 80 prior to introduction to the mixer 60, with effluent from the dewatering apparatus 80 optionally transferred to a save-all tank 90 for the return of recovered wet fiber 30 to the pulper 40. The at least partially dewatered partitioned fibers or the partitioned fibers that have not been dewatered are transferred directly to the mixer 60 or they may optionally be disentangled by being fluffed and/or chopped in apparatus 100 further disentangling the fibers prior to introduction to the mixer 60. In addition or alternatively, the fibers are agitated directly within the mixer 60 by chopper blades or other mechanical action that may serve as another mechanism to further disentangle the fibers while still at least partially moist or wet. The fundamental function of the chopper 100 is to disentangle the fibers in a wet state so that they are not clumped together but are disentangled into more individual fibers and/or smaller clumps of fibers, which clumps are smaller than clumps existing before reaching the mixer 60. While the fibers may have been originally partitioned and disentangled in an upstream pulping process, the process of at least partially dewatering under pressure can have the effect of re-entangling fibers together, and the chopper 100 can be useful in re-disentangling the fibers from one another. Because the chopper 100 operates on fibers still in the wet state, breakage of the fibers is again minimized. If superstructures of fibers are present while material is being chopped, the chopper 100 may be tuned to maintain the integrity of a specific scale of superstructures, while disentangling other larger clumps, for example. That tuning may be accomplished by selectable spacing between individual chopping blades, for example.

[0036] The fibers, whether all fibers or those of the first stream previously described, are mixed in the mixer 60 with one or more fire retardancy chemical compounds 110 and one or more solvents. The one or solvents may be water, another liquid, or a combination of water and another liquid. The solvent may either be added to the mixer 60 or it may come with the partitioned fibers in the transfer from any one of the pulper 40, the partitioning device 50, the dewatering apparatus 80 and the disentanglement apparatus 100. The one or more fire retardancy chemical compounds may be added to the mixer 60 before, during or after introducing the partitioned and optionally disentangled fibers to the mixer 60. Optionally, one or more additives 120 may be added to the mixer 60 before, during or after introducing the fibers to the mixer 60. The one or more additives 120 may be used to enhance the characteristics of the fibers to improve fire retardancy chemical attachment on and in the fibers. For example, the additives may include one or more enzymes suitable to remove residual adhesive from the recycled feedstock material 10. One or more bonding agents 130 may also be added to the mixer 60 before, during or after introducing the partitioned and optionally disentangled fibers to the mixer 60. The one or more bonding agents 130 may be selected to cause individual fibers to clump together and remain joined together. The bonding agents may be added at the mixer 60 or may be applied in downstream processes and may cause the joining to occur in the mixer 60 or at a downstream stage, such as during drying. The bonding between fibers may form fiber superstructures with interstices between the fibers that improve the insulative characteristics of the finished product.

[0037] The fibers, the one or more fire retardancy chemical compounds 110, and any optional additives and/or bonding agents contained in the mixer 60 are mixed together for a sufficient amount of time for the fire retardancy chemical compounds to be retained on and in the fibers, and to enable sufficient fiber bonding to occur before completion of processing if it is a goal to form fiber superstructures in the mixer 60. Treated fibers exiting the mixer 60 are transferred to a drying apparatus 140 to be dried to a liquid content in the range of about 5% to about 25% by weight. Optionally, the treated fibers may first be pressed in a pressing apparatus 150. The pressing apparatus 150 may have the function of removing water, helping to form a plurality of superstructures, or both functions. Optionally, the treated and dried fibers may be fiberized in fiberizer 170. The treated and dried fibers may further optionally be classified in dry classifier 180, either directly from the drying apparatus 140 or from the optional fiberizer 170. The purpose of the dry classifier 180 is to ensure that the properties of the finished product meet the targeted characteristics for size, density and/or hydrodynamic diameter. The dry classifier may provide as outputs both the desired product and non-conforming materials, which may include dust (smaller than desired particles) or larger clumps (heavier than desired materials). Following optional classification, a selected subset of treated and dried fibers may then be in satisfactory form to be packaged for use as a a fire-retardant cellulose insulation 160 made as described herein. It is noted that the fire-retardant cellulose insulation 160 may be a standalone insulation product or it may be a component of a composite insulation product containing one or more other components not made in the manner described with respect to the making of the fire-retardant cellulose insulation 160.

[0038] When the optional dry classifier 180 is employed, non-conforming materials such as small particles and dust 190, or large and heavy materials 195, may be removed from treated and dried fibers that are the desired product and returned to the mixer 60 or to another stage of the process. Dust may be returned for agglomeration when the one or more bonding agents 130 are in the mixer 60 and/or the small particles and dust 190 may be returned to one or more other apparatuses for reconstitution as fiber superstructure components of the finished end product 160. The small particles and dust 190 may optionally be diverted to an agglomeration apparatus 200, which may simply be a dry mixer, for combining with one or more supplemental bonding agents 210 and/or other supplemental fibers 220 to form additional residual fiber superstructures that may be added to the treated and dried fibers as the end product 160.

[0039] The feedstock material 10 may be one or more recyclable materials that are cellulose-based, including, but not limited to any plant-based materials. Additional fiber feedstocks suitable for use in the invention include sources of agriculturally derived fibers, such as cereal straw, animal feathers, and other lignocellulosic agricultural byproducts, for example. The virgin feedstock material 20 may be from a kraft or a groundwood (stone or thermo-mechanical). The ratio of feedstock material 10 to virgin material 20 and/or recovered wet fibers 30 is selectable when the combination is used. The feedstock material(s) may be added to the partitioning device 50 at a level of 1% to 30% solids by weight.

[0040] As noted, the virgin feedstock material 20 can be hardwood (1.5 mm), softwood (3.5 mm) (resulting from the kraft process) or groundwood (<1 mm) (includes stone, thermo-mechanical process), and/or cellulose pulp fibers, which may be diverted from a conventional cellulose processing system prior to bleaching, or immediately afterward if that is of interest. Pulp coming off the last black liquor washer in a kraft process, for example, before going into the bleaching process (20% solid by weight) can be used. A pump may be used to move pulped fibers from the pulper 40 to the partitioning device 50. Those of skill in the art will recognize that any sort of material transfer mechanism may be used to move material including, but not limited to, pulped material from one location to another for the process of the present invention.

[0041] Recycled newsprint pulp may be obtained from a conventional paper recycle process, such as from ONP #8 and #9 sources, for example. The paper can be introduced into the pulper 40. The pulper 40 is a tank that has an agitator and a source of solvent, such as water, to pulp the feedstock. The agitation disentangles the fibers and breaks down the cellulosic material into fiber stalks. The one or more fire retardants 110 may be delivered to the mixer 60 in liquid form, such as by being dissolved in a solvent such as water. The fire retardants 110 when combined with fibers in a liquid environment are better adhered to the surface of and absorbed into the structure of the fibers than when dry fire retardancy chemicals are applied to the exterior of dry fibers. The addition of fire retardants to wet fibers in a mixer can also provide better absorption and better uniformity of distribution as compared to when liquid fire retardancy chemicals are simply sprayed onto dry feedstock such as paper rather than fibers in a moist state, particularly fibers that may have been disentangled prior to or during the mixing operation. The fire retardant can be in a dry or a wet form combined with fiber in wet form or it can be combined in dry or wet form with fibers and the one or more solvents. The one or more fire retardants may be selected from boric acid, borax, ammonium sulfate, monoammonium phosphate, diammonium phosphate, sodium tetraborate, ferrous sulfate, magnesium sulfate, zinc sulfate and mixtures thereof. An example of a suitable fire retardancy chemical composition is described in U.S. Pat. No. 8,043,384, the content of which is incorporated herein by reference.

[0042] The chemical saturation, operating temperature, and dwell time in the mixer 60 is selectable to ensure that the finished cellulose insulation contains a sufficient amount of fire-retardancy material adhered in and to the fibers of the insulation. The one or more retardants dissolved in solvent can range from 1% to 50% solids content. The contents of mixer 60 can be combined at in a temperature range from 25 C to 80 C. The mixer may actively agitate the contents of mixer 60 for a period ranging from 5 sec to 30 minutes, after which, the material may be allowed to dwell and homogenize in the mixer or a subsequent storage or conveyance system for a period of 5 minutes to 48 hours. The one or more other additives may be used to hydrolyze starch, polysaccharide, or other undesirable materials, for example, as well as one or more biocides, as desired to minimize mold growth in the end product 160. The chemicals, additives and/or bonding agents may be mixed together before transfer to the mixer 60 such as with a mixing valve, or they may be transferred separately to the mixer 60.

[0043] The optional dewatering apparatus 80 is selected from any number of existing systems that take a cellulose pulp slurry and remove water to a desired solids content. Any type of screw press, twin wire press, vacuum filter, plate and frame press, roll press, or centrifugal drum, for example, can be used as the dewatering apparatus 80. The optional dewatering system 80 may increase the solids content of the slurry containing the treated fibers to about 30% or more but not limited thereto.

[0044] A pump or other form of material transfer mechanism can be used to transfer dewater effluent to the save-all 90, which separates fibers from fluid. This can be accomplished by a flotation, rotary (vacuum filters) or wire (fabric) system that can efficiently remove the fluid. The fibers from the save-all are moved to the recovered wet fiber container 30. Excess fluid from the save-all 90 can be filtered for use in other process components of the system or put into a waste treatment process for removal.

[0045] The optional fluffer/chopper 100 is configured to break up a pulp cake of treated fibers or optionally at least partially dewatered treated fibers. The fluffer/chopper 100 can be two counter rotating meshed blades with a discharge to the drying system 140. Any number of fluffers can be used to break up the pulp cake. The pulp cake can be broken up ahead of the mixer 60 or internally within the mixer 60 by blades internal to the mixer that may be designed to disentangle fibers.

[0046] The drying system 140 is used to dry the treated fibers down to a desired moisture content, which may range from 8-25% in moisture content (75-92% solids), for example, but not limited thereto. A dryer, such as but not limited to, a rotary drum dryer or flash dryer system that breaks up and fluffs the pulp while drying may be advantageous, but other drying systems such as microwave dryers and conveyorized dryers may also be employed. A belt conveyor, auger system or other form of conveyance device may be used to transport the dried and chemically treated fibers to a location for cooling. An exhaust gas/hot air collection system from the dryer system may be employed to take moist air and recirculate it back through the drying system 140 to capture residual heat before exhausting to the atmosphere.

[0047] An optional dry fluffer 165 may be used to disentangle clumps of materials that may have formed in the drying process, while minimally affecting the basic structure of the fibers and while retaining desired fiber superstructures when such superstructures form part of the end product. Alternatively, an optional fiberizer 170 may be used as a more aggressive measure to further refine the treated and dried fibers, by further disentangling fiber clusters, reducing the size of the fibers clusters, individuating fibers, and fibrillating fibers after the drying process. Those partially disentangled or fully disentangled fibers and/or fiber superstructures may optionally be further partitioned by size using the dry classifier 180. The dry fluffer 165 and the fiberizer 170 can be mechanical devices with rotating toothed plates in close proximity to one or more sets of static or counter rotating toothed plates such that when clumps of fibers are conveyed through the device 165/170, they are subjected to shear forces which can disentangle clumps of fibers and may also individuate fibers and fibrillate fibers. The distinction between a fluffer and a fiberizer is in the severity of their interaction with the materials, with a fluffer more gently disentangling groups or clumps of fibers and a fiberizer more aggressively impacting the materials with greater shear.

[0048] A hammer mill is an example of a fiberizer, but there are also fiberizers formed with one or more rotating toothed plates in close proximity to one or more stationary or counterrotating toothed plates. Traditional fiberizers used to make cellulose insulation with dry fire retardants mix the chemical and fiber in a high velocity grinding motion, which can have the effect of pressing chemicals onto the fibers and creating adhesion. While this process can be used to meet regulatory requirements, the dust can come off during installation, creating a dusty work environment and impeding visibility. The method of the present invention takes the treated fibers with the absorbed chemicals and dries them as individual fibers or clumped together into desired superstructures. Because the fire retardant is inside the fibers, the present invention dramatically reduces the amount of chemical dust produced during installation.

[0049] The optional chopper 100 may be used instead of the optional fiberizer 170 but it is used prior to drying the treated fibers. In that way, dust formation is reduced as compared to when the fiberizer 170 is used after drying. The use of the chopper 100 breaks up the clumps in a way that is different from the fiberizing and post-drying disentanglement processes described above. Specifically, because the fibers are moist, they are more pliable and less susceptible to breakage. Further, fibers may be combined with one or more binders to form superstructures before chopping. The binder may be a chemical additive suitable for joining fibers together, and a suitable binder may be a starch, adhesive, or other binder. These superstructures may have spaced bonds between fibers and/or fiber particulates that establish voids for improving insulative and density characteristics and those bonds may be formed directly or through use of an optional binder. The use of the chopper 100 instead of the fiberizer 170 can improve the likelihood of maintaining superstructure integrity because the fibers are more pliable and less fragile in a moist or wet state.

[0050] Treated and dried fibers may optionally be sent for testing. Testing may be performed on the fibrous material that is the cellulose insulation of the present invention for compliance with all regulations concerning blown-in cellulosic fiber insulation as directed by the C-739, HH 1515, and the Consumer Product Safety Council. The treated fibers made using the method of the present invention can be used as a fire retardant, thermal, sound and radiant barrier material for insulating.

[0051] In addition to being used to partition fibers with differing characteristics, the partitioning device 50 can also intentionally divide streams of contaminants from streams containing the desired fibers from the feedstocks. These contaminants of the recycled feedstock material 10 may include glass, plastic or other non-cellulose elements, for example. The partitioning device 50 may be comprised of a screening system, or a cyclonic separator, which are two examples of partitioning technologies that may be applicable. The partitioning device 50 may additionally include or instead be a screening apparatus such as the type shown at: https://www.andritz.com/products-en/group/pulp-and-paper/pulp-production/kraft-pulp/pulp-drying-finishing/pulp-screening-cleaning, for example, to facilitate fiber classification prior to introducing the feedstock material into the mixer 60.

[0052] The optional dry classifier 180 may be used to partition by size treated and dried fibers so that relatively small particulates that are effectively dust particles are removed from the product to minimize dust inclusion in the finished product. The dry classifier 180 may be a screening apparatus or an air classifier. An air classifier may use an upward airflow to partition lighter elements from heavier elements, for example. The dry classifier 180 may operate to partition fibers based on size, density, hydrodynamic diameter or other characteristics. For example, the dry classifier 180 may be utilized to select fibers, which may be critical in producing high performing product, and to reject less desirable fractions of the processed materials, such as heavy contaminants like sand, glass, and metal, which would otherwise degrade the properties of the finished product. Alternatively, a dry classifier 180 may also be utilized to reject lighter fractions of a stream such as dust, so that dust is rejected and excluded from the finished product, while fibers are accepted and conveyed forward to the finished product.

[0053] Examples of the product of the present invention were made using the method of the present invention as described herein. Fibers were disentangled via a pulping process and then partitioned using a classification system, subsequently being treated with fire resistant chemicals, mixed with other fiber sources and dried to produce finished product. The finished product was tested against ASTM C739 and found to be fully compliant. The product was provided to installers in the field and found to be a high quality finished product that was low in dust.

[0054] The present invention of methods for providing an improved fire-retardant material and, in particular, a cellulose insulation fabrication and the cellulose insulation made thereby, have been described with respect to specific components and method steps. Nevertheless, it is to be understood that various modifications may be made without departing from the spirit and scope of the invention. All equivalents are deemed to fall within the scope of this description of the invention as identified by the following claims.