Method of manufacturing polarizing plastic lens
10099439 ยท 2018-10-16
Assignee
Inventors
- Masaki Ihara (Nagano, JP)
- Hiroshi Shimizu (Nagano, JP)
- Yoshinobu Ito (Nagano, JP)
- Toshihiko Shimizu (Nagano, JP)
- Kenichi Tonouchi (Nagano, JP)
Cpc classification
B29C39/10
PERFORMING OPERATIONS; TRANSPORTING
B29C39/24
PERFORMING OPERATIONS; TRANSPORTING
B29D11/00413
PERFORMING OPERATIONS; TRANSPORTING
B29K2629/04
PERFORMING OPERATIONS; TRANSPORTING
International classification
B29D11/00
PERFORMING OPERATIONS; TRANSPORTING
B29C39/24
PERFORMING OPERATIONS; TRANSPORTING
Abstract
Method of manufacturing polarizing plastic lens, including an upper mold positioning step of positioning an upper mold so that a nonmolding surface faces up and a molding surface faces down, an adhesive column forming step of discharging a thixotropic curable adhesive from a nozzle beneath the upper mold to form adhesive columns on the molding surface of the upper mold, a step of bonding the upper mold and a polarizing film, an adhesive column curing step of subjecting the adhesive columns to a curing treatment, a casting mold assembling step of assembling a casting mold having a cavity within which the polarizing film has been positioned with the upper mold to which the polarizing film has been bonded, a lower mold positioned opposite the upper mold so as to sandwich the polarizing film, and a sealing member maintaining a spacing between the upper mold and lower mold, and a polymerizing and curing step of casting a curable composition into the cavity, and polymerizing and curing the curable composition that has been cast to provide a polarizing plastic lens within which the polarizing film is positioned.
Claims
1. A method of manufacturing a polarizing plastic lens, which comprises: an upper mold positioning step of positioning an upper mold so that a nonmolding surface faces up and a molding surface faces down; an adhesive column forming step of discharging a thixotropic curable adhesive, from a discharge nozzle positioned beneath the molding surface of the upper mold, at 8 to 50 spots on a rim portion of the molding surface of the upper mold, and repeating the discharging of the thixotropic curable adhesive at each of the multiple spots to form adhesive columns, wherein during the discharging, the discharge nozzle is displaced downward, or the upper mold is displaced upward, or the discharge nozzle is displaced downward and the upper mold is displaced upward, to adjust a spacing between a tip of each of the adhesive columns and a tip of the discharge nozzle; a bonding step of bonding the upper mold and a polarizing film by means of the adhesive columns that have been formed; an adhesive column curing step of subjecting the adhesive columns to a curing treatment after the bonding step; a casting mold assembling step of assembling a casting mold having a cavity within which the polarizing film has been positioned with the upper mold to which the polarizing film has been bonded, a lower mold positioned opposite the upper mold so as to sandwich the polarizing film, and a sealing member maintaining a spacing between the upper mold and lower mold; and a polymerizing and curing step of casting a curable composition into the cavity, and polymerizing and curing the curable composition that has been cast to provide a polarizing plastic lens within which the polarizing film is positioned.
2. The method of manufacturing a polarizing plastic lens according to claim 1, wherein the thixotropic curable adhesive has a thixotropy coefficient of equal to or greater than 2.
3. The method of manufacturing a polarizing plastic lens according to claim 1, wherein the thixotropic curable adhesive has a viscosity of equal to or greater than 30,000 mPa.Math.s.
4. The method of manufacturing a polarizing plastic lens according to claim 1, wherein the thixotropic curable adhesive has a thixotropy coefficient of equal to or greater than 2.5 and a viscosity of equal to or greater than 35,000 mPa.Math.s.
5. The method of manufacturing a polarizing plastic lens according to claim 1, which further comprises a step of curved surface processing the polarizing film and wherein the polarizing film that is bonded to the upper mold is a polarizing film that has been curved surface processed.
6. The method of manufacturing a polarizing plastic lens according claim 1, wherein the thixotropic curable adhesive is a photosetting adhesive and the adhesive column curing step is conducted by irradiating light.
7. The method of manufacturing a polarizing plastic lens according to claim 1, wherein, in the casting mold assembling step, the upper mold and the lower mold are positioned so as to sandwich the polarizing film across a prescribed distance, and the cavity of the casting mold includes a first cavity formed between the upper mold and the polarizing film and a second cavity formed between the lower mold and the polarizing film.
8. The method of manufacturing a polarizing plastic lens according to claim 7, wherein the curable composition is cast into the cavity through a casting hole provided on the second cavity side of the casting mold.
9. The method of manufacturing a polarizing plastic lens according to claim 1, wherein, in at least one of the upper mold positioning step and the adhesive column forming step, the nonmolding surface of the upper mold is held with a vacuum pad.
10. The method of manufacturing a polarizing plastic lens according to claim 1, wherein, in the bonding step, the bonding of the upper mold and the polarizing film is conducted while vacuum suction is applied to the polarizing film.
11. The method of manufacturing a polarizing plastic lens according to claim 1, wherein the adhesive columns have a height in a range of from 0.1 mm to 1.0 mm.
12. A method of manufacturing a polarizing plastic lens, which comprises: an upper mold positioning step of positioning an upper mold so that a nonmolding surface faces up and a molding surface faces down; an adhesive column forming step of discharging a thixotropic curable adhesive from a discharge nozzle positioned beneath the molding surface of the upper mold to form adhesive columns on a rim portion of the molding surface of the upper mold; a bonding step of bonding, while vacuum suction is applied to the polarizing film, the upper mold and a polarizing film by means of the adhesive columns that have been formed; an adhesive column curing step of subjecting the adhesive columns to a curing treatment after the bonding step; a casting mold assembling step of assembling a casting mold having a cavity within which the polarizing film has been positioned with the upper mold to which the polarizing film has been bonded, a lower mold positioned opposite the upper mold so as to sandwich the polarizing film, and a sealing member maintaining a spacing between the upper mold and lower mold; and a polymerizing and curing step of casting a curable composition into the cavity, and polymerizing and curing the curable composition that has been cast to provide a polarizing plastic lens within which the polarizing film is positioned.
13. The method of manufacturing a polarizing plastic lens according to claim 12, wherein the thixotropic curable adhesive has a thixotropy coefficient of equal to or greater than 2.
14. The method of manufacturing a polarizing plastic lens according to claim 12, wherein the thixotropic curable adhesive has a viscosity of equal to or greater than 30,000 mPa.Math.s.
15. The method of manufacturing a polarizing plastic lens according to claim 12, wherein the thixotropic curable adhesive has a thixotropy coefficient of equal to or greater than 2.5 and a viscosity of equal to or greater than 35,000 mPa.Math.s.
16. The method of manufacturing a polarizing plastic lens according to claim 12, which further comprises a step of curved surface processing the polarizing film and wherein the polarizing film that is bonded to the upper mold is a polarizing film that has been curved surface processed.
17. The method of manufacturing a polarizing plastic lens according claim 12, wherein the thixotropic curable adhesive is a photosetting adhesive and the adhesive column curing step is conducted by irradiating light.
18. The method of manufacturing a polarizing plastic lens according to claim 12, wherein, in the adhesive column forming step, the thixotropic curable adhesive is discharged at multiple spots of 8 to 50 spots on the rim portion of the molding surface of the upper mold, and the discharging of the thixotropic curable adhesive at each of the multiple spots is repeated to form the adhesive columns.
19. The method of manufacturing a polarizing plastic lens according to claim 18, wherein, during the discharging, the discharge nozzle is displaced downward, or the upper mold is displaced upward, or the discharge nozzle is displaced downward and the upper mold is displaced upward, to adjust a spacing between a tip of each of the adhesive columns and a tip of the discharge nozzle.
20. The method of manufacturing a polarizing plastic lens according to claim 12, wherein, in the casting mold assembling step, the upper mold and the lower mold are positioned so as to sandwich the polarizing film across a prescribed distance, and the cavity of the casting mold includes a first cavity formed between the upper mold and the polarizing film and a second cavity formed between the lower mold and the polarizing film.
21. The method of manufacturing a polarizing plastic lens according to claim 20, wherein the curable composition is cast into the cavity through a casting hole provided on the second cavity side of the casting mold.
22. The method of manufacturing a polarizing plastic lens according to claim 12, wherein, in at least one of the upper mold positioning step and the adhesive column forming step, the nonmolding surface of the upper mold is held with a vacuum pad.
23. The method of manufacturing a polarizing plastic lens according to claim 12, wherein the adhesive columns have a height in a range of from 0.1 mm to 1.0 mm.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1)
(2)
(3)
(4)
(5)
(6)
(7)
(8)
(9)
(10)
(11)
(12)
(13)
MODES FOR CARRYING OUT THE INVENTION
(14) The present invention will be described through specific implementation modes below with reference to the drawings. However, the present invention is not limited to the embodiments shown in the drawings. Portions described in the drawings have been shown suitably enlarged or reduced so as to be identifiable.
(15) <Structure of Polarizing Plastic Lens>
(16) The structure of the polarizing plastic lens will be described below with reference to the drawings.
(17)
(18) In this context, in polarizing plastic lens 100, polarizing film 14 desirably faces convex surface 111 and is convex in shape. Since polarizing film 14 can be positioned along the shape of convex surface 111 in this manner, the polishable thickness of lens substrate 120 can be increased relative to the case where polarizing film 14 is of a convex shape facing concave surface 121. Accordingly, the thickness of the lens obtained as a finished product can be reduced.
(19) Lens substrates 110 and 120 are desirably plastic lenses with refractive indexes of equal to or higher than 1.50. The materials of lens substrates 110 and 120 are not specifically limited. Examples are acrylic resins, polyurethane resins, thiourethane resins, thioepoxy resins, methacrylic resins, allyl resins, episulfide resins, and polycarbonate resins. From the perspective of reducing thickness, thiourethane resins and thioepoxy resins are desirable. From the perspective of ease of coloration, urethane resins are desirable. Lens substrate 110 and lens substrate 120 are desirably comprised of the same material. Lens substrate 110 and lens substrate 120 can be dyed to impart color.
(20) Polarizing film 14 is desirably either a single layer or a multilayer film equipped with a resin layer comprised of polyvinyl chloride (PVA). PVA is a good material in terms of transparence, heat resistance, affinity with dyes in the form of iodine or dichroic dyes, and orientation properties during stretching. For example, film 14 can be a film-like substrate obtained by press molding, vacuum molding, or the like a commercial iodine polarizing film to conduct curved surface processing to a specified curvature, and cutting into a round external shape. Curved surface processing will be described below.
(21) A multilayer polarizing film 14 can be obtained by molding a film in which PVA is impregnated with iodine, to form a resin layer that has been uniaxially stretched, and then laminating a protective layer in the form of triacetylcellulose (TAC) on both surfaces of the resin layer. It is also possible to employ a polarizing film fabricated using a dichroic dye instead of iodine. It is also possible to employ a single layer polarizing film in the form of PVA on which a TAC protective film has not been laminated, or a polarizing film employing polyethylene terephthalate (PET) instead of PVA. In the present implementation mode, a polarizing film 14 of PVA without lamination of protective layers of TAC is employed. Polarizing film 14 is colored to impart a predetermined color, such as brown or gray.
(22) <Structure of Lens Monomer Infusion Machine>
(23) An example of a lens monomer infusion machine that can be used to cast the curable composition (also referred to as a lens monomer) into the cavity of the casting mold will be described next based on the drawings.
(24)
(25) Lens monomer infusion machine 2 relating to the present implementation mode is equipped with a positioning member 10, an suctioning member 19, and a feeding member 24, as shown in
(26) Multiple holding members 11 are positioned in positioning member 10. Holding members 11 hold casting mold 12.
(27) As shown in
(28) The type of material (inorganic, organic) of mold 13 is not specifically limited beyond that it be a material capable of withstanding heating in the manufacturing of polarizing plastic lens 100. In the present implementation mode, crown glass is employed in mold 13. Transparent organic substances (such as resins) deteriorate when irradiated with ultraviolet radiation, and are thus not suitable for use in a casting mold that molds large numbers of polarizing plastic lenses 100. However, for example, they can be used in casting molds for molding small numbers of sample product or the like by exploiting the cost advantage.
(29) Polarizing film 14 is applied with an adhesive column 20 to upper mold 131.
(30) In casting mold 12, without using a gasket, upper mold 131 and lower mold 132 are positioned with a prescribed gap between them such that molding surfaces 131A and 132A are facing each other, and adhesive tape 46 is wound over the entire circumference of the outer edges of upper and lower molds 131 and 132. In this manner, a cavity 50 enclosed by upper mold 131, lower mold 132, and adhesive tape 46 is formed.
(31) In a portion of adhesive tape 46 is formed an casting hole, not shown, for casting lens monomer into cavity 50. This casting hole can be formed after casting mold 12 is held with pressing members 11 and mounted on positioning member 10, or can be formed by machining a hole in part of adhesive tape 45 during the forming of casting mold 12.
(32) In
(33) Suctioning tube 23 is shaped in the form of a tube and is positioned such that the tip of the tube is positioned near the casting hole. Suctioning tube 23 is connected to recovery member 31, suctions starting material composition that spills out of the casting hole of casting mold 12, and feeds it to recovery member 31.
(34) Recovery member 31 recovers and stores the lens monomer that has been suctioned by suctioning tube 23. Further, recovery member 31 is equipped with a pump, not shown. Lens monomer is suctioned from suctioning tube 23 by suitably controlling this pump.
(35) Feeding member 24 is equipped with a feeding member main body 21, a storage member 40, and a casting member 25.
(36) Feeding member main body 21 is connected to storage member 40 and guides the lens monomer that enters from storage member 40 to casting member 25. A control element, not shown, is electrically connected to feeding member main body 21. The configuration can be such that the quantity of lens monomer that is fed into casting member 25 is adjusted by controls effected by this control element. Casting member 25 is equipped with a casting needle, not shown, that can be inserted into the casting hole provided in adhesive tape 46 of casting mold 12, and casts lens monomer that is fed by feeding member main body 21 into cavity 50 of casting mold 12.
(37) Storage member 40 is connected to feeding member main body 21 and feeds lens monomer. A composition of a monomer of an isocyanate compound or an isothiocyanate compound having two or more isocyanate groups or isothiocyanate groups per molecule, and a monomer of a thiol compound having two or more mercapto groups per molecule, can be employed in the present implementation mode as the lens monomer fed from storage member 40. A composition containing a monomer of a thioepoxy compound can also be employed as the lens monomer. Intermediates of polymerization reactions, such as prepolymers, can be included in the lens monomer in addition to, or instead of, the monomers.
(38) <Method of Manufacturing a Polarizing Plastic Lens>
(39) The method of manufacturing polarizing plastic lens 100 of the present implementation mode will be described based on the drawings.
(40)
(41) <Polarizing Film Molding Step>
(42)
(43) As shown in
(44) The curved surface processing of the polarizing film that can be desirably conducted in the method of manufacturing a polarizing plastic lens relating to an embodiment of the present invention will be described next.
(45) Of the two lens substrates that sandwich the polarizing film, one has a convex surface and the other has a concave surface. By positioning the polarizing film within the casting mold following curved surface processing, it is possible to embed the polarizing film between the two lens substrates along the curved surface shape of the lens. Curved surface processing is desirably conducted by the press molding method such that the polarizing film is made to correspond to the molding surface shape (concave surface shape) of the upper mold.
(46) For example, a flat sheet of polarizing film is sandwiched and pressed in a press molding device having a shaping mold (master mold) with a pair consisting of a male mold and a female mold equipped with a temperature-adjusting means (heater, cooling medium, or the like) and a pressurizing means to conduct curved surface processing of the polarizing film into the shape of the surface of the shaping mold. Male and female molds with spherical molding surfaces are desirably employed. Because of the spherical surfaces and lack of complex shapes, a special pressing device is not required, a normal press molding device will suffice, and curving is facilitated.
(47)
(48) The curvature of the curved surface of master mold part 261 is set based on the base curve of the refractive surface on the convex surface side of the lens being manufactured.
(49) A flat film member 210 that has been cut into rectangular shape out of a polarizing polyvinyl alcohol film is placed on the male mold of the master mold part and pressed, for example, at room temperature (about 20 to 25 C.) with a pressing means having the female mold, not shown, of the master mold part to transfer the shapes of curved surfaces 212a and 212b to the polarizing film and obtain a polarizing film having curved surfaces 214a and 214b.
(50) Prior to conducting curved surface processing, it is desirable to wet the polarizing film to enhance the shape-transferring property to the master mold part. The wetting treatment can be conducted, for example, by a method such as placing the polarizing film for a prescribed period in a constant-humidity, high-temperature device, spraying water in the form of a mist onto the polarizing film, and the like. The wetting can be conducted in a heated atmosphere of about 50 to 90 C.
(51) In order to conduct curved surface processing in a state in which most of the water absorbed will be retained in the film, cooling of the wetted polarizing film is desirable. For example, a polarizing film that has been removed from a constant-humidity, high-temperature device can be placed as is at room temperature (about 20 to 25 C.) to cool the polarizing film.
(52) In a desirable embodiment, the polarizing film that has been curved surface processed is heated to a heating temperature of equal to or higher than 105 C. but lower than 150 C. The heating temperature of the polarizing film that has been curved surface processed is the temperature of the atmosphere at which the heat treatment is conducted. The polarizing film that has been curved surface processed can be heated prior to being placed in the casting mold to prevent deformation of the polarizing film. As a result, deformation of the surface of the polarizing plastic lens, particularly the surface on the object side, can be prevented. Here, employing a heating temperature of equal to or higher than 105 C. can prevent deformation well and employing a temperature of lower than 150 C. can prevent the occurrence of discoloring and distortion of the polarizing film. The heating temperature is desirably equal to or higher than 120 C., and desirably equal to or lower than 130 C. This heat treatment can be conducted in air.
(53) Various heating methods can be adopted. In one implementation mode, the polarizing film is placed in a hot air-circulating oven that has been heated to the temperature set forth above and exposed to a hot air flow. Heating is conducted until the polarizing film shrinks adequately.
(54) As shown in
(55) As shown in
(56) It is possible to obtain a polarizing plastic lens in which a curved surface processed polarizing film has been sandwiched between two lens substrates by placing the polarizing film that has been curved surface processed as set forth above in a casting mold, and molding a lens by the casting method. The polarizing plastic lens is normally surface processed, edge processed, and mounted into a frame to obtain eyeglasses or sunglasses equipped with polarizing plastic lenses as set forth above.
(57) <Assembling of Casting Mold>
(58) The casting mold is assembled through a step of positioning an upper mold, a step of forming adhesive columns, a step of bonding the upper mold and the polarizing film, a step of curing the adhesive columns, and a step of assembling the casting mold. Prior to the step of positioning the upper mold, it is also possible to conduct a step of measuring the depth of the concave surface of upper mold 131 and the center height of polarizing film 14.
(59) Each of these steps will be described in order below.
(60) (Measuring Step)
(61)
(62)
(63) (Upper Mold Positioning Step and Adhesive Column Forming Step)
(64)
(65) Discharge device 22 relating to the present implementation mode is equipped with an X cylinder 27 moving in a direction perpendicular to the direction in which gravity acts (also referred to as the horizontal direction, hereinafter); a Z cylinder 29 moving vertically in the direction in which gravity acts (also referred to as the vertical direction, hereinafter), a spindle 33 supported by X cylinder 27 and Z cylinder 29; a dispenser 35, and a syringe 36.
(66) A flexible vacuum pad 37 is positioned beneath spindle 33 (
(67) Dispenser 35 positioned beneath the molding surface of the upper mold discharges upward adhesive that has been loaded in advance into syringe 36, thereby forming adhesive columns 20. Dispenser 35 is controlled by dispenser control element 39, discharging adhesive 20 in a constant discharge quantity through nozzle 38. Concave surface 131A is facing downward. Thus, adhesive column 20 that is formed at the position of discharge of concave surface 131A sags downward. For example, in the method of discharging an adhesive with a concave surface facing upward, disclosed in above-cited Japanese Unexamined Patent Publication (KOKAI) No. 2009-3303 and Japanese Unexamined Patent Publication (KOKAI) No. 2012-198689 disclose, the adhesive builds up due to countering the effect of gravity. Thus, adhesive becomes a lump, topping or tilting, sometimes not reaching the height prescribed by the design. When adhesive column 20 does not reach the prescribed height, it becomes difficult to position polarizing film 14 within polarizing plastic lens 100, it becomes impossible to stably hold the polarizing film, and the quality of the exterior appearance is compromised. Further, when one of the surfaces of polarizing plastic lens 100 is polished (processed), the thickness that can be polished without scratching polarizing film 14 decreases, and the thickness of the finished product lens that is obtained sometimes ends up being thicker than the thickness of an eyeglass lens not containing polarizing film 14. By contrast, by having concave surface 131A facing downward and forming adhesive column 20, gravity causes adhesive column 20 to sag downward. That makes it possible to more reliably and precisely achieve a prescribed height in adhesive column 20. Thus, it becomes possible to obtain a thinner finished product polarizing lens with a better external appearance. For example, it becomes possible to obtain a polarizing lens that can be suitably employed as a semifinished eyeglass lens. Multiple spindles 33 and dispensers 35 can be provided in discharge device 22, and a configuration that discharges multiple adhesive columns 20 on upper mold 131 is possible in a single discharge device 22. An example of dispenser 35 is the jet type dispenser Aerojet (Aerojet is a registered trademark) made by Musashi Engineering, Inc.
(68) The method of forming adhesive column 20 employing discharge device 22 will be described next.
(69) Once upper mold 131 has been positioned, dispenser 35 discharges adhesive onto the outer circumference portion of upper mold 131. As shown in
(70) Discharge device 22 discharges adhesive until adhesive column 20 reaches a prescribed height (length). The height (length) of adhesive column 20 at a given discharge position refers to the distance between the top of adhesive column 20 and the point of intersection with concave surface 131A of a vertical line run downward to concave surface 131A from this top. The height of the adhesive column can be determined based on the height at which one desires to maintain polarizing film 14. For example, in the case where the curvature of film 14 is identical to the curvature of concave surface 131A, it is desirably equal to or higher than 0.1 mm but equal to or less than 1.0 mm. By keeping it to equal to or higher than 0.1 mm but equal to or less than 1.0 mm, it is possible to achieve a minimum value of the distance between polarizing film 14 on polarizing plastic lens 100 and the convex surface 111 of within a range of equal to or higher than 0.1 mm but equal to or less than 1.0 mm. With the minimum value of the distance between polarizing film 14 and convex surface 111 is equal to or higher than 0.1 mm but equal to or less than 1.0 mm, when manufacturing a finished product lens by polishing the concave surface side of the lens, the thickness (thickness of the thinnest portion) of the finished product lens that is obtained can be made a lens thickness of equal to or less than 1.1 mm, which is equivalent to the thickness of an eyeglass lens not containing polarizing film 14. Accordingly, it is possible to achieve a thickness that is equivalent to an eyeglass lens not containing polarizing film 14 in an eyeglass lens containing polarizing film 14. For example, the adhesive column has a rod shape or a shape approximating a rod. However, this is not a limitation. It can have any lump shape, such as a square rod.
(71) When the height 82 of the center of polarizing film 14 is greater than the concave portion depth 80 of upper mold 131 (when the radius of curvature of polarizing film 14 is smaller than that of upper mold 131), the spacing is controlled based on the center of upper mold 131 and polarizing film 14. In this case, it is because the center portion of polarizing film 14 ends up contacting upper mold 13 when the spacing is determined based on the outer circumference. When the height 82 of the center of polarizing film 14 is less than the concave portion depth 80 of upper mold 131 (when the radius of curvature of polarizing film 14 is greater than that of upper mold 131), the spacing is controlled based on the outer circumference portion of upper mold 131 and polarizing film 14. In this case, this is because when the spacing is determined based on the center, the outer circumference of polarizing film 14 ends up coming into contact with upper mold 131. When the concave portion depth 80 of upper mold 131 equals the height 82 at the center of polarizing film 14, it suffices to adjust the spacing anywhere. The top that is employed in an eyeglass lens or the area around the top is desirably employed as a reference.
(72) Further, when polarizing film 14 is bonded in the manner described further below to adhesive column 20 of prescribed height, the top will sometimes be slightly quashed, changing the height. In that case, the height of adhesive column 20 is desirably set in advance to a height that is increased by the amount of the reduction in height due to bonding of polarizing film 14.
(73) In the present implementation mode, a single discharge device discharges adhesive multiple times to adjust the amount of adhesive that is discharged at a particular position. To reliably form adhesive column 20 of prescribed height, the discharge nozzle is desirably positioned straight down at the spot where the adhesive column is to be formed. It is preferable for adhesive to be discharged directly upward through the discharge nozzle thus positioned. The angle between concave surface 131A and the direction of discharge of the adhesive is desirably constant at the multiple spots where adhesive columns are to be formed. This can inhibit variation in the height of adhesive columns 20 at various spots when identical quantities of adhesive are discharged.
(74) The height of adhesive column 20 can be controlled by adjusting the quantity of adhesive that is discharged at the spots where adhesive columns are to be formed. In order not to adhere adhesive in spots where the formation of an adhesive column is not wanted, a gap is desirably provided between nozzle 38 and the concave surface 131A. That is, it is desirable for adhesive droplets to be scattered through nozzle 38 in conducting the discharge. The quantity of adhesive that is discharged through nozzle 38 each time can be reduced. However, the greater the quantity of the adhesive that is discharged, the harder it becomes to scatter adhesive in the form of adhesive droplets.
(75) To ensure an effective diameter (the size of the area that can be utilized as an eyeglass) in the finished product polarizing lens, the position at which adhesive column 20 is formed is the rim portion of upper mold 131, desirably to the outside of the effective diameter of the finished product polarizing lens that is obtained when processing polarizing plastic lens 100. The position at which adhesive column 20 is formed can be a region that is removed in a lens rounding step or the like that removes the bur or adjusts the shape of the rim portion of molded polarizing plastic lens 100 to a circular shape, or can be a region of the lens rim portion that remains. It suffices for it to be a region that is cut when the lens is mounted into a frame that has been selected by a customer. When adhesive column 20 does not affect the optical performance of the finished product polarizing lens, it is possible to form the adhesive column within the effective diameter. The diameter of adhesive column 20 is desirably the smallest diameter capable of holding polarizing film 14 from the perspectives of facilitating mold release, cleaning upper mold 131 after mold release, and the minimization of the amount of the outer circumference portion (edge surface) of polarizing plastic lens 100 that is shaped. The diameter of the adhesive column can be adjusted based on the inner diameter of the opening of nozzle 38. For example, the diameter desirably falls within a range of 1.0 to 2.0 mm. To prevent scattering of adhesive and the reliable buildup of adhesive at desired positions, the distance between upper mold 131 and the dispenser discharge outlet is desirably equal to or less than 50 mm, preferably equal to or less than 30 mm. When dispenser 35 repeatedly dispenses adhesive, adhesive deposits near the opening of nozzle 38, compromising discharge performance. Thus, it is desirable to regularly clean the area around the opening of nozzle 38. This cleaning can be conducted by the method of suctioning away unwanted adhesive by means of a vacuum. It can also be conducted by wiping with a sponge, cloth, or paper. In addition to manual operations, it is possible to add a cleaning mechanism to discharge device 22. Making a blank shot prior to discharging onto upper mold 131 can yield a stable discharge from the beginning.
(76) As set forth above, in discharging the adhesive, displacing the discharge nozzle downward is desirable to adjust the spacing between the tip of the adhesive column and the tip of the discharge nozzle. To this end, either one or both of the upper mold and the discharge nozzle are displaced. For example, the longer the adhesive column, the more the discharge nozzle is displaced downward or the more the upper mold is displaced upward to keep the spacing between tip of the adhesive column and the tip of the discharge nozzle constant. In this case, it is desirable to move the adhesive in a direction in which the angle of discharge relative to concave surface 131A does not change.
(77) The adhesive that is used to form the adhesive column will be described next.
(78) The adhesive that is employed to form the adhesive column is both thixotropic and curable. This can prevent deformation of the adhesive column and make it possible to precisely control the gap between the upper mold and the polarizing film, that is, the spacing from the convex surface to the polarizing film in the polarizing plastic lens being manufactured, by means of the height of the adhesive column. Details are as set forth above.
(79) The use of an adhesive with a thixotropy coefficient of equal to or greater than 2 is desirable, greater than 2 is preferred, equal to or greater than 2.5 is of greater preference, and equal to or greater than 3 is of still greater preference. The thixotropy coefficient is, for example, equal or less than 5. The greater the thixotropy, the better from the perspective of maintaining the shape of the adhesive columns. Thus, there is no upper limit. From the perspective of better retaining the shape of the adhesive column, the viscosity of the adhesive is desirably equal to or greater than 30,000 mPa.Math.s, preferably equal to or greater than 35,000 mPa.Math.s. The greater the viscosity, the better from the perspective of shape retention. From the perspective of ease of coating, an adhesive with a viscosity of equal to or less than 100,000 mPa.Math.s is desirable, one with a viscosity of equal to or less than 80,000 mPa.Math.s is preferred, and one with a viscosity of equal to or less than 70,000 mPa.Math.s is of greater preference. As regards curability, an adhesive exhibiting a thermosetting property of curing when heated or an adhesive exhibiting a photosetting property of curing when irradiated with light will do. From the perspective of manufacturing efficiency, a short curing period is desirable. Thus, a photosetting adhesive is desirably employed. For example, an ultraviolet-curable adhesive can be suitably employed. The adhesive can be a composition, containing, for example, a prepolymer, monomer, photopolymerization initiator, some other polymerization initiator, and additives. Because the adhesive column comes into contact with the lens monomer that is positioned within the cavity of the casting mold, an adhesive that satisfies the conditions of not dissolving into the lens monomer and not causing monomer foaming due to the generation of gas or the like is desirable. Examples of adhesives that can be suitably employed are thixotropic ultraviolet-curable acrylic resin compositions.
(80) The position of the formation of the adhesive column will be described next.
(81)
(82) The adhesive columns are formed, for example, by discharging with a dispenser an adhesive in the form of a thixotropic ultraviolet-curable resin composition. The adhesive is discharged in multiple spots on the outer circumference portion, which is the rim, of the concave surface 131A of upper mold 131. The present implementation mode shows the embodiment of adhesive discharge at 32 spots on the outer circumference portion. The position of the adhesive discharge depends on the type of polarizing film. By way of example, there can be two or more spots, desirably four or more spots. When there are fewer than four spots, polarizing film 14 will curl in spots that have not been secured with adhesive. In some cases, it is impossible to maintain all of polarizing film 14 at a prescribed height relative to polarizing plastic lens 100.
(83) For example, when adhesive columns are formed in about 32 spots on a polarizing plastic lens (semifinished lens) for use in high optical precision eyeglasses for refractive correction that have a lens diameter of about 65 to 80 mm, bending of the polarizing film can be kept so low as to be almost visually undetectable. In a lens about 65 to 80 mm in diameter, in terms of restrictions relating to the surface area available for discharge, the high end of the number of spots where adhesive columns are formed is normally about 50. It is desirable for the adhesive columns in the cavity not to impede the flow of lens monomer to allow the smooth filling of the cavity of the casting mold with lens monomer. Thus, the number of spots in which adhesive columns are formed, by way of example, is desirably about 8 to 50, preferably 16 to 40. When the number of spots in which adhesive columns are formed is excessive, adjacent adhesive columns end up joining together, sometimes impeding the flow of lens monomer.
(84) When forming adhesive columns in multiple spots, it is desirable for there to be little variation in the spacing between spots, and identical spacing is preferred. That is, the adhesive columns are desirably formed at an equal spacing on the rim portion of the molding surface of the upper mold. This can facilitate maintaining all of polarizing film 14 at a prescribed height.
(85) (Bonding Step)
(86)
(87) (Adhesive Column Curing Step)
(88)
(89) (Casting Mold Assembling Step)
(90) The upper mold and the polarizing film are bonded through adhesive columns in the above steps. As shown in
(91) In the course of positioning lower mold 132, lower mold 132 is positioned opposite polarizing film 14 so that the thickness of cavity 50 (the distance between lower mold 132 and upper mold 131) assumes a set thickness. That is, upper mold 131 and lower mold 132 are positioned so as to sandwich polarizing film 14 across a prescribed distance. Lower mold 132 is a round, platelike member made of glass. The convex surface 132A of lower mold 132 is curved so as to mold the concave surface 121 of the polarizing plastic lens 100 that is being molded.
(92) The material of adhesive tape 46 is not specifically limited. From the perspectives of ease of use and economy, a plastic adhesive tape is desirably employed. For example, adhesive tape 46 with a base material made of polypropylene or polyethylene terephthalate combined with one or more adhesives in the form of an acrylic, natural rubber, or silicon adhesive can be prepared. Casting holes for introducing lens monomer can be provided in adhesive tape 46. Winding adhesive tape 46 onto the circumferential surface of lower mold 132 and upper mold 131 which have been positioned opposite each other constitutes casting mold 12 comprised of upper mold 131 and lower mold 132, which sandwich polarizing film 14, and adhesive tape 46.
(93) <Casting Step>
(94)
(95) <Curing Step>
(96) Following the casting step, casting mold 12 filled with lens monomer is placed in a heating furnace and heated. Here, the heating temperature is desirably 0 to 150 C., preferably 10 to 130 C. The temperature is desirably raised over 5 to 50 hours, preferably over 10 to 25 hours, and polymerization is conducted. For example, 30 C. is maintained for 7 hours, after which the temperature is raised from 30 to 120 C. over 15 hours.
(97) <Mold Release Step>
(98) Next, once the heat treatment has been concluded, a polarizing plastic lens 100 in which a polarizing film 14 is embedded is manufactured (see
(99) As set forth in detail above, in the present implementation mode, the molding surface of the upper mold and polarizing film 14 are brought into contact through adhesive columns 20 which sag downward in the direction in which gravity acts. Adhesive columns 20 are solidified with the concave surface 131A of upper mold 13 and polarizing film 14 separated by a prescribed gap to secure polarizing film 14 to the concave surface 131A of upper mold 13. Since a prescribed spacing can be maintained between polarizing film 14 and the convex surface 111 of polarizing plastic lens 100 that is being manufactured, a polarizing plastic lens 100 with an external appearance of good quality can be obtained. Although a sealing member in the form of adhesive tape has been employed in the implementation mode set forth above, the same effect can be achieved when a gasket is employed instead of tape. That is, without providing a configuration (grooves, tabs, or the like) on a gasket to hold polarizing film 14, it is possible to hold polarizing film 14 within casting mold 12 with a prescribed gap between the molding surface of upper mold 13 and polarizing film 14 and obtain a polarizing plastic lens 100 with an external appearance of good quality.
(100) A further aspect of the present invention relates to a device of manufacturing a polarizing plastic lens employing the manufacturing method that has been set forth in detail above. The configuration of the device is as described above. The details of the various components of the device are as set forth above for the manufacturing method.
(101) The four adhesives shown in Table 1 below were used to form adhesive columns on the rim portions of the molding surface of an upper mold in the above implementation mode. After forming adhesive columns, the bonding step and adhesive column curing step were implemented based on the above implementation mode to bond the upper mold to the polarizing film (Tests 1 to 4). Tests 1 to 4 were conducted under identical conditions with the exception that the adhesives were varied.
(102) As Test 5, lens monomer was discharged downward onto the molding surface of an upper mold with its molding surface facing upward through a discharge nozzle that was positioned above the molding surface to form adhesive columns based on the implementation mode described in above-cited Japanese Unexamined Patent Publication (KOKAI) No. 2012-198389 using adhesive A. Subsequently, the upper mold and the polarizing film were bonded based on the implementation mode described in the same publication.
(103) In these tests 1 to 5, adhesive columns 1.0 to 2.0 mm in diameter were formed in 32 spots as shown in
(104) In each of the tests, the height of the adhesive columns positioned between the upper mold and the polarizing film was measured. Evaluation was conducted by determining how close the average value of the height measured in 32 spots was to the targeted height of the adhesive columns (setting value) according to the following evaluation scale. The results are given in Table 1.
(105) <Evaluation Scale>
(106) A: Setting value down to 10% (range permitting extremely precise control of the setting height) B: Setting value 11% to 20% (range permitting precise control of the setting height) C: Setting value 21% to 30% D: Setting value 31% and below E: Tilting and toppling of adhesive columns occurred
(107) TABLE-US-00001 TABLE 1 Test 5 (Adhesive applied downward Test 1 Test 2 Test 3 Test 4 from above) Type of Adhe- Adhe- Adhe- Adhe- Adhe- adhesive sive A sive B sive C sive D sive A Thixotropy 3 to 4 3 to 4 2.0 1 to 1.5 3 to 4 coefficient Viscosity 52,000 35,000 30,000 60,000 52,000 mPa .Math. s Evaluation A A C D E results (control of height of adhesive column) Adhesive A: Ultraviolet-curable acrylic resin composition World Rock 8840H2 made by Kyoritsu Chemical & Co., Ltd. Adhesive B: Ultraviolet-curable acrylic resin composition World Rock 8172H2 made by Kyoritsu Chemical & Co., Ltd. Adhesive C: Ultraviolet-curable acrylic resin composition World Rock XVL90T3 made by Kyoritsu Chemical & Co., Ltd. Adhesive D: Ultraviolet-curable acrylic resin composition World Rock XB06 made by Kyoritsu Chemical & Co., Ltd.
(108) Study on heating temperature of polarizing film after curved surface processing
(109) <Fabrication of Sample Lens 1>
(110) 1. Wetting Treatment of Polarizing Film, Curved Surface Processing, and Subsequent Heat Treatment
(111) A commercial dichroic dye polymerizing film made of PVA was placed in a constant humidity high temperature device and subjected to a wetting treatment. It was wetted to a moisture content of about 4% at the start of the curved surface processing. The wetted polarizing film was placed for about 2 minutes at room temperature (20 to 25 C.) and then curved surface processed by the method set forth above based on
(112) Next, the curved surface processed polymerizing film was heated for 30 minutes at 120 C. in a commercial hot air recirculating oven. The heating was conducted without a curved surface processing base (glass mold) 260.
(113) 2. Molding and Mold Release of Lens by Casting Polymerization Method
(114) A 50.6 g quantity of m-xylene diisocyanate and 49.4 g of 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane were admixed as plastic lens starting materials and thoroughly stirred.
(115) To this were added 1.2 g of a UV absorbing agent sold as SEESORB701 (made by Cipro Chemical Industries) and 0.1 g of an internal mold release agent sold as MR internal mold release agent (made by Mitsui Chemical Corp.). Mixing was followed by thorough stirring. To the fully dispersed or dissolved plastic lens starting materials was added a catalyst in the form of 100 ppm of dibutyltin dichloride. The mixture was thoroughly stirred at room temperature to obtain a uniform liquid. This composition was subjected to reduced pressure of 5 mmHg and degassed while being stirred for 30 minutes to fabricate a lens monomer.
(116) The lens monomer that had been prepared was cast into a casting mold having positioned in the interior thereof the polarizing film after the heating treatment of 1. above. The upper mold and lower mold had surfaces that were spherical in shape, inner diameters of 80 mm, and radii of curvature of 130.4 mm.
(117) Subsequently, the casting mold was placed in a heating furnace and a temperature of 30 C. was maintained for 7 hours. Subsequently, the temperature was raised from 30 to 120 C. over 10 hours and heat curing was conducted.
(118) Following the heat curing, the casting mold was removed from the heating furnace and the lens was removed from the casting mold to obtain a lens (semifinished lens). The concave surface of this lens was ground/polished with a curve generator and polishing apparatus to obtain an eyeglass lens for vision correction in accordance with a prescription.
(119) <Evaluation of Optical Performance of Lens>
(120) After mold release, to evaluate deformation of the lens (in a round uncut state), the optical performance was evaluated based on the following items. Visual examination was implemented by inspectors with three years or more of experience in lens inspection operations. The evaluation results are given in Table 2.
(121) (1) Shape Deformation
(122) The maximum radius of curvature (mm) (Rmax) at the position of the geometric center of the convex surface of the lens (=optical center) and the minimum radius of curvature (mm) (Rmin) were measures with a FOCOVISON radius of curvature measuring device (made by Automation & Robotics).
(123) The difference in curvature (RmaxRmin) of the maximum radius of curvature (mm) and minimum radius of curvature (mm) was adopted as an indicator of deformation (astigmatism) of the lens and evaluated as set forth below. The convex surface of the lens was of spherical design. The geometric center of the convex surface is the point of intersection of a perpendicular line passing through the center of the circle when the lens is viewed from above and the side of the convex surface of the lens.
(124) A difference in curvature of 0 or more but less than 3 mm was evaluated as: (passing); 3 mm or more but less than 4 mm as: (some deformation seen but no impediment for use in eyeglasses); 4 mm or more: (practical impediments).
(125) (2) Discoloration of Polarizing Film
(126) The presence or absence of discoloration of the polarizing film in the lens was visually determined. No discoloration: Coloration of a degree presenting no change in hue observed: Discoloration presenting a clearly different hue:
(3) Distortion of Polarizing Film
(127) Distortion (deformation of surface shape) of the polarizing film within the lens was visually (by inspectors with three or more years of experience in lens inspection operations) determined. No distortion observed at all: Distortion observed in some of the rim portions of the lens, but no practical problems presented for eyeglasses: Readily apparent distortion:
(128) Overall Evaluation
(129) A lens that received no for lens deformation, discoloration of polarizing film, or distortion of polarizing film was evaluated as , and a lens that received at least one was evaluated as . Lenses that received in all evaluated items were evaluated as .
(130) <Sample Lenses 2 to 5 and Reference Lenses 1 to 4>
(131) With the exception that heating of the polarizing films that had been curved surface processed was conducted under the conditions given in Table 2, various sample lenses and reference lenses were fabricated in the same manner as Sample Lens 1. Reference Lens 1 was employed without heating the polarizing film.
(132) <Sample Lenses 6 and 7, Reference Lenses 5 and 6>
(133) With the exceptions that a commercial laminated polarizing film (TAC/PVA) having TAC protective layers on both surfaces of a dichroic dye polarizing film made of PVA was employed instead of using commercial dichroic dye polarizing film made of PVA in the fabrication of Sample Lens 1 and heating of the polarizing film was conducted under the conditions given in Table 2, various sample lenses and reference lenses were fabricated in the same manner as Sample Lens 1.
(134) <Sample Lens 8>
(135) With the exception that the polarizing film was held by the curved surface processing base 60 used in the curved surface processing to conduct heating, a lens was fabricated in the same manner as in the fabrication of Sample Lens 2.
(136) TABLE-US-00002 TABLE 2 Condition of heating polarizing film Heating Heating Rmax Discoloration of Distortion of Polarizing Glass temperature time Rmax Rmin Rmin Lens polarizing polarizing Overall film mold ( C.) (hour) (nm) (nm) (nm) deformation film film evaluation Sample Lens 1 PVA None 120 0.5 129 127.9 1.1 Sample Lens 2 PVA None 120 2 129 126.3 2.7 Sample Lens 3 PVA None 130 2 129.7 126.9 2.8 Sample Lens 4 PVA None 105 2 130.1 126.6 3.5 Sample Lens 5 TAC/PVA None 140 2 128.9 128.1 0.8 Sample Lens 6 TAC/PVA None 120 2 129 127.8 1.2 Sample Lens 7 PVA None 140 2 129.2 128 1.2 Sample Lens 8 PVA Employed 120 2 129 127.7 1.3 Referene Lens 1 PVA None 135.7 127.9 7.8 X X Referene Lens 2 PVA None 60 5 136.1 128.1 8 X X Referene Lens 3 PVA None 100 5 132.4 127.8 4.6 X X Referene Lens 4 PVA None 150 2 129.5 128 1.5 X X Referene Lens 5 TAC/PVA None 100 2 136.5 126.5 10 X X Referene Lens 6 TAC/PVA None 150 2 129.5 128 1.5 X X
(137) As shown in Table 2, Sample Lens 4, which was obtained by heating a curved surface processed polarizing film to 105 C., had a difference in radius of curvature (RmaxRmin) of 3.5 mm. Sample Lenses 5 and 7, which were obtained by heating the polarizing film to 140 C., exhibited discoloration of a degree that did not present a change in hue. However, both of these sample lenses could be practically used without impediment as polarizing lenses.
(138) Heating to 120 to 130 C. was found to yield less lens deformation and polarizing film discoloration, and to yield a lens with good optical performance and good external appearance.
(139) Both Sample Lenses 6 and 7, in which were employed laminated polarizing films, produced similar results. Thus, the use of a polarizing film that had been heated under similar conditions was found to inhibit shape deformation of the lens, not just in PVA films, but also in other films.
(140) By contrast, in Reference Lenses 1 to 3 and Reference Lens 5, the difference in radius of curvature (RmaxRmin) was 4 mm or greater. The lenses presented considerable shape deformation. Reference Lenses 1 to 3 and Reference Lens 5 were all obtained using heating temperatures of less than 105 C. and were thought to not have undergone adequate shrinkage of the polarizing film prior to casting of the composition capable of polymerization for lens substrates. Thus, the polarizing film was thought to have shrunken during thermosetting, deforming the lens.
(141) Deformation of the lens was inhibited due to heating of the polarizing film to 150 C. in Reference Lenses 4 and 6, but the polarizing film underwent degeneration and discoloration.
(142) Sample Lenses 1 to 7, for which curved surface processing base 260 was not employed, exhibited distortion in the shape of the polarizing film, although slight, but Sample Lens 8, for which curved surface processing base 260 was employed, exhibited suppression of distortion in the form of a lens presenting good optical performance.
(143) Accordingly, holding the polarizing film on curved surface processing base 260 to conduct heating was found to suitably inhibit shape deformation and distortion of the polarizing film and yield a lens of better external appearance.
(144) Based on the above results, heating a lens that has been curved surface processed to a prescribed temperature was determined to provide a polarizing plastic lens with little deformation of lens surface shape that causes astigmatism.
(145) In addition, heating a curved surface processed polarizing film while holding it on the curved surface processing base 260 used in curved surface processing can inhibit change in the curved surface portion 261a (see
(146) By combining the above-described curved surface processing and method of manufacturing a polarizing lens set forth in detail above, it is possible to provide a polarizing lens of extremely high quality with both inhibited deformation of the lens surface shape and inhibited reduction of external appearance quality that are caused by deformation of the adhesive columns and the like.
INDUSTRIAL APPLICABILITY
(147) The present invention is useful in the field of manufacturing eyeglasses and eyeglass lenses.