Press-forming tool and method for manufacturing press-formed product
09878362 ยท 2018-01-30
Assignee
Inventors
Cpc classification
B21D53/88
PERFORMING OPERATIONS; TRANSPORTING
B21J5/00
PERFORMING OPERATIONS; TRANSPORTING
B21D5/01
PERFORMING OPERATIONS; TRANSPORTING
B21D22/26
PERFORMING OPERATIONS; TRANSPORTING
B21D24/04
PERFORMING OPERATIONS; TRANSPORTING
B21D22/22
PERFORMING OPERATIONS; TRANSPORTING
International classification
B21D22/26
PERFORMING OPERATIONS; TRANSPORTING
B21D22/22
PERFORMING OPERATIONS; TRANSPORTING
B21D5/01
PERFORMING OPERATIONS; TRANSPORTING
B21J5/00
PERFORMING OPERATIONS; TRANSPORTING
Abstract
A press-forming tool comprising: a punch including a punch portion and a plate portion transferring shape to a blank material; a die paired with the punch and opposes the punch portion; a wrinkle suppression mold including a first surface opposing the plate portion and comes into contact with the plate portion at a press-forming ending point, a second surface opposing the die and holds the blank material along with the die, and a third surface continued between the first and second surface and opposes the punch portion, and disposed between the third surface and the punch portion via a gap; a pressure receiving portion including a groove portion on the first surface of the wrinkle suppression mold; and a wrinkle suppression force increasing portion disposed on a surface opposing the first surface of the plate portion, protrudes toward the pressure receiving portion, and generates a reaction force opposed to a pressing direction when pressed in the pressing direction in end-phase of a press-forming.
Claims
1. A press-forming tool comprising: a punch which includes a punch portion and a plate portion which are configured to transfer a shape to a blank material; a die which is paired with the punch and which opposes the punch portion; a wrinkle suppression mold which includes a first surface which opposes the plate portion and which comes into contact with the plate portion at a press-forming ending point, a second surface which opposes the die and which holds the blank material along with the die, and a third surface which is continuous between the first surface and the second surface and which opposes the punch portion via a gap; a pressure receiving portion which includes a groove portion and which is disposed on the first surface of the wrinkle suppression mold, the groove portion having a depth greater than zero with respect to the first surface of the wrinkle suppression mold; and a wrinkle suppression force increasing portion which is disposed on the plate portion so as to oppose the first surface, which protrudes toward the pressure receiving portion, which does not contact the groove portion of the pressure-receiving portion at a press-forming starting point, and which generates a reaction force in a direction opposite to a pressing direction when being pressed in the pressing direction in an end phase of a press forming.
2. The press-forming tool according to claim 1, wherein when a region in which a plate thickness is maximum in a flange portion of a press-formed product is defined as a plate thickness maximum portion and a region in which the plate thickness is more than 0% and less than or equal to 97% with respect to the plate thickness maximum portion is defined as a plate thickness decreasing portion, based on a case where the pressure receiving portion and the wrinkle suppression force increasing portion are removed from the press-forming tool, the pressure receiving portion overlaps with a portion of a region corresponding to the plate thickness decreasing portion in the blank material when viewed along the pressing direction.
3. The press-forming tool according to claim 1, wherein the pressure receiving portion is consisted of the groove portion, when a thickness of the wrinkle suppression mold in a position of the groove portion is defined as L in mm units and a minimum value of the thickness of the wrinkle suppression mold in a position which excludes the groove portion and comes into contact with the blank material is defined as H in mm units, the wrinkle suppression mold satisfies a following Expression 1 or 2, and when a protruding height of the wrinkle suppression force increasing portion is defined as G in mm units and a press stroke distance from the press-forming starting point to the press-forming ending point is defined as PS in mm units, and the protruding height G of the wrinkle suppression force increasing portion satisfies a following Expression 3:
20L0.8H when 40H50(Expression 1)
20L40 when 50<H80(Expression 2)
0.02PS+HLG0.3PS+HL(Expression 3).
4. The press-forming tool according to claim 1, wherein a portion of a boundary which partitions the pressure receiving portion is the groove portion.
5. The press-forming tool according to claim 1, wherein the wrinkle suppression force increasing portion includes an elastic body which applies the reaction force.
6. The press-forming tool according to claim 5, wherein the elastic body is at least one of a disc spring, a helical spring, and a rubber.
7. A method for manufacturing a press-formed product which is press-formed using the press-forming tool according to claim 1, comprising: press-forming a blank material by increasing a wrinkle suppression force with respect to a portion of the blank material in an end phase of a press forming, which is started at a position at which a press stroke is 2% to 30% and which is ended at a forming end position, when a forming start position of the press stroke is defined as 100% and the forming end position of the press stroke is defined as 0% during the press forming of the blank material.
8. The press-forming tool according to claim 2, wherein the pressure receiving portion is consisted of the groove portion, when a thickness of the wrinkle suppression mold in a position of the groove portion is defined as L in mm units and a minimum value of the thickness of the wrinkle suppression mold in a position which excludes the groove portion and comes into contact with the blank material is defined as H in mm units, the wrinkle suppression mold satisfies a following Expression 1 or 2, and when a protruding height of the wrinkle suppression force increasing portion is defined as G in mm units and a press stroke distance from the press-forming starting point to the press-forming ending point is defined as PS in mm units, and the protruding height G of the wrinkle suppression force increasing portion satisfies a following Expression 3:
20L0.8H when 40H50(Expression 1)
20L40 when 50<H80(Expression 2)
0.02PS+HLG0.3PS+HL(Expression 3).
9. The press-forming tool according to claim 2, wherein a portion of a boundary which partitions the pressure receiving portion is the groove portion.
10. The press-forming tool according to claim 2, wherein the wrinkle suppression force increasing portion includes an elastic body which applies the reaction force.
11. The press-forming tool according to claim 10, wherein the elastic body is at least one of a disc spring, a helical spring, and a rubber.
12. A method for manufacturing a press-formed product which is press-formed using the press-forming tool according to claim 2, comprising: press-forming a blank material by increasing a wrinkle suppression force with respect to a portion of the blank material in an end phase of a press forming, which is started at a position at which a press stroke is 2% to 30% and which is ended at a forming end position, when a forming start position of the press stroke is defined as 100% and the forming end position of the press stroke is defined as 0% during the press forming of the blank material.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1)
(2)
(3)
(4)
(5)
(6)
(7)
(8)
(9)
(10)
(11)
(12)
(13)
(14)
(15)
(16)
(17)
(18)
(19)
(20)
(21)
(22)
(23)
(24)
(25)
(26)
(27)
(28)
(29)
(30)
(31)
(32)
(33)
(34)
(35)
(36)
(37)
EMBODIMENTS OF THE INVENTION
(38) Hereinafter, each embodiment of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to only the configurations of the following embodiments, and various modifications may be applied to the present invention within a scope which does not depart from the gist of the present invention. Moreover, in the drawings used for the following description, in order to make the description easier to be understood, for convenience, a portion becoming a main portion may be shown to be enlarged, and it is not limited that a dimension ratio of each component or the like is the same as the actual condition.
(39)
(40) The press-forming tool 1 according to the present embodiment includes a punch 10, a die 20, and wrinkle suppression molds 25a and 25b. The punch 10 includes a punch portion 12 and a plate portion 14 configured to transfer a shape to a blank material. The punch portion 12 and the plate portion 14 are fixed to each other by a fastening member (not shown) and become the punch 10. Alternatively, the punch portion 12 and the plate portion 14 may integrally form the punch 10.
(41) As shown in
(42) The die 20 is paired with the punch 10 and is disposed so as to oppose the punch portion 12. The wrinkle suppression molds 25a and 25b are disposed between the punch 10 and the die 20. The wrinkle suppression molds 25a and 25b according to the present embodiment are constituted of the minimum number of components, which is difficult to divide it further, from the viewpoint of a structure of a press mold and a shape of a press-formed product. That is to say, the wrinkle suppression molds 25a and 25b are not split-type wrinkle suppression molds but integral-type wrinkle suppression molds.
(43) The wrinkle suppression molds 25a and 25b include first surfaces 31a and 31b which oppose the plate portion 14 of the punch 10 and which come into contact with the plate portion 14 at a press-forming ending point. In addition, the wrinkle suppression molds 25a and 25b include second surfaces 32a and 32b which oppose the die 20 and which hold the blank material along with the die 20.
(44) A side surface (third surface) 33a which is continuous between the first surface 31a and the second surface 32a oppose the punch portion 12 via a predetermined gap (clearance). Similarly, a side surface (third surface) 33b which is continuous between the first surface 31b and the second surface 32b oppose the punch portion 12 via a predetermined gap (clearance). By setting the gap appropriately, occurrence of wrinkles of the press-formed product or cracks of the press-formed product can be preferably prevented. The setting of the gap may be determined according to a routine procedure.
(45)
(46)
(47) A blank material 5 is disposed on the second surfaces 32a and 32b of the wrinkle suppression molds 25a and 25b in a state where the second surfaces 32a and 32b of the wrinkle suppression molds 25a and 25b and a tip surface 13 of the punch portion 12 are flush with each other.
(48) As shown in
(49) Moreover, as shown in
(50) At a predetermined position in the end phase of the press forming, the pressure receiving portions 30a and 30b provided on the first surfaces 31a and 31b of the wrinkle suppression molds 25a and 25b come into contact with the wrinkle suppression force increasing portions 16a and 16b. Moreover, the pressure receiving portions 30a and 30b press the wrinkle suppression force increasing portions 16a and 16b in the pressing direction in conjunction with the press forming from the predetermined position of the end phase of the press forming to the press-forming ending point.
(51) As a result, the reaction force in the direction opposite to the pressing direction is generated from the wrinkle suppression force increasing portions 16a and 16b. The pressure receiving portions 30a and 30b receive the reaction force, and the wrinkle suppression force with respect to the blank material 5 in the end phase of the press forming is increased.
(52)
(53) As shown in
(54) Instead of the disc spring 42a, an elastic body such as a helical spring or a rubber may be used. It is preferable that the disc spring 42a is used since it is possible to obtain a high load even by a low stroke.
(55) As shown in
(56) As a result, the reaction force is transmitted to the blank material 5 which is held between the second surface 32a of the wrinkle suppression mold 25a and the die 20, and thus, the wrinkle suppression force with respect to the blank material 5 can be increased in the end phase of the press forming.
(57) The wrinkle suppression mold 25a which receives the reaction force from the disc spring 42a includes the pressure receiving portion 30a which is constituted of a groove portion, and thus, the wrinkle suppression mold 25a is convexly and elastically deformed to the blank material 5 side and is bent. That is to say, when viewed along the pressing direction, a portion which is convexly and elastically deformed on the second surface 32a corresponding to the pressure receiving portion 30a effectively transmits the reaction force to the blank material 5. Here, the pressure receiving portion 30a is formed on the first surface 31a of the wrinkle suppression mold 25a.
(58) If the wrinkle suppression mold 25a does not include the pressure receiving portion 30a, the reaction force from the disc spring 42a is distributed to the entire wrinkle suppression mold 25a. Accordingly, since the reaction force cannot be locally applied to the blank material 5, the transmission efficiency of the reaction force is decreased.
(59)
(60) In the press-forming tool 1 according to the present embodiment, the thickness H is constant. However, when the thickness is not constant, the minimum value of the thickness on the region which excludes the pressure receiving portion 30a and comes into contact with the blank material 5 may be set to H. For example, as the case where the thickness H is not constant, there is a case where a press-formed product in which the height of the flange surface is not constant is formed, as shown in
(61) The lower limit of the thickness L is preferably set to 20 mm. If the thickness L is less than 20 mm, the wrinkle suppression mold 25a may be plastically deformed or damaged during drawing and bending processing (during press forming).
(62) On the other hand, in the case of 40H50, the upper limit of the thickness L is preferably set to 0.8H. If the thickness L exceeds 0.8H, even when the pressure receiving portion 30a receives the reaction force from the wrinkle suppression force increasing portion 16a, the wrinkle suppression mold 25a is not elastically deformed, and thus, the reaction force may not be effectively transmitted to the blank material 5.
(63) In the case of 40H50, the preferable upper limit of the thickness L is 0.6H. If the upper limit of the thickness L is 0.6H, even when capability of the wrinkle suppression force increasing portion 16a is small, the reaction force generated by the wrinkle suppression force increasing portion 16a can be effectively transmitted to the blank material 5.
(64) In the case of 50<H80, the upper limit of the thickness L is preferably set to 40 mm regardless of the thickness H. The maximum value of the reaction force, which is received from the wrinkle suppression force increasing portion 16a to the pressure receiving portion 30a, is 6.5 MPa. Accordingly, if the thickness L exceeds 40 mm, stiffness of the pressure receiving portion 30a is increased, and the wrinkle suppression mold 25 may not be elastically deformed even by the maximum value of the reaction force.
(65) If the thickness H is less than 40 mm, the stiffness of the entire wrinkle suppression mold 25a is not sufficient. On the other hand, if the thickness H exceeds 80 mm, the stiffness of the wrinkle suppression mold 25a is increased more than necessary, and a material cost of the wrinkle suppression mold 25a is also increased.
(66) In summary about the thicknesses of the wrinkle suppression mold 25a, a relationship between the thickness L and the thickness H preferably satisfies the relationship of the following Expression 1 or 2. Moreover, although it is not shown, the wrinkle suppression mold 25b is also similar to the above.
20L0.8H when 40H50(Expression 1)
20L40 when 50<H80(Expression 2)
(67) The reaction force from the wrinkle suppression force increasing portion 16a is generated from contacting the pressure receiving portion 30a provided on the wrinkle suppression mold 25a with the pin 40a, until the pressure receiving portion 30a reaches the press-forming ending point. The position of contacting the pressure receiving portion 30a provided on the wrinkle suppression mold 25a with the pin 40a may be a predetermined position in the end phase of the press forming. The position of contacting the pressure receiving portion 30a with the pin 40a may be controlled by changing the protruding length (height) of the tip of the pin 40a from the surface of the plate 14.
(68) As shown in
(69) The protruding height of the tip of the pin 40a of the wrinkle suppression force increasing portion 16a from the surface of the plate 14 is defined as G in mm units. A press stroke distance from a press-forming starting point, which is a press stroke position at which the plastic deformation of the blank material 5 starts, to the press-forming ending point is defined as PS in mm units. At this time, the protruding height G of the wrinkle suppression force increasing portion 16a may preferably satisfy the following Expression 3. Moreover, although it is not shown, the wrinkle suppression force increasing portion 16b is also similar to the above.
0.02PS+HLG0.3PS+HL(Expression 3)
(70) The protruding height G of the pin 40a is preferably equal to or more than a value which adds the groove depth (HL) of the pressure receiving portion 30a to 2% of the press stroke distance PS (0.02PS). That is to say, the interval of the press stroke which increase the wrinkle suppression force in the end phase of the press forming is preferably equal to or more than 2% of the press stroke distance PS.
(71) If the protruding height G is less than the value (0.02PS+HL), the increase of the wrinkle suppression force is not sufficient, and the effects which is exerted by decreasing the springback may be unstable. In order to further decrease the springback, the value of the protruding height G is preferably equal to or more than (0.05PS+HL).
(72) On the other hand, it is preferable that the protruding height G of the pin 40a be less than or equal to a value which adds the groove depth (HL) of the pressure receiving portion 30a to 30% of the press stroke distance PS (0.3PS). That is to say, the interval of the press stroke which increases the wrinkle suppression force in the end phase of the press forming is preferably less than or equal to 30% of the press stroke distance PS.
(73) If the protruding height G exceeds the value (0.3PS+HL), since the interval of increasing the wrinkle suppression force becomes too long, a difference in the wrinkle suppression force becomes smaller between the press-forming starting point and the press-forming ending point. Accordingly, the effect which is exerted by increasing the wrinkle suppression force is decreased only in the end phase of the press forming is decreased, and thus, the springback may occur to the contrary. In order to further decrease the springback, the value of the protruding height G is preferably less than or equal to (0.15PS+HL).
(74) So far, it is mainly described regarding the wrinkle suppression mold 25a and the wrinkle suppression force increasing portion 16a. However, the wrinkle suppression mold 25b and the wrinkle suppression force increasing portion 16a are similar to the above.
(75)
(76) The press-formed product 50 includes flange portions 54a and 54b, vertical wall portions 55a and 55b, and a top portion 55c. Moreover, straight side portions 51a and 51b and a bent portion 52 interposed between the straight side portions 51a and 51b are provided on both ends of the press-formed product 50.
(77) When viewed from the cross section perpendicular to the longitudinal direction, the press-formed product 50 has a so-called hat-shaped cross section, and both ends in the longitudinal direction of the press-formed product 50 are opened. Here, when viewed from an arrow A direction in
(78) When the press forming is performed, according to the shape of the press-formed product 50, it is generated that a portion in which a plastic flow of the blank material 5 is easily occurred and a portion in which the plastic flow is not easily occurred. According to a difference in ease of the generation of the plastic flow, non-uniformity of residual stress in a plate thickness direction or an in-plane direction of the press-formed product 50 occurs.
(79) Moreover, due to the non-uniformity of the residual stress, for example, springback such as warpage, twist, or waviness of the vertical wall portions 55a and 55b occurs on the press-formed product 50. Particularly, when the shape of the press-formed product 50 has a curved portion, shrinkage flange deformation or extension flange deformation is applied in the longitudinal direction of the press-formed product 50. Accordingly, the non-uniformity of the residual stress in the plate thickness direction or the in-plane direction is increased.
(80) In general, after the drawing and bending processing is performed, finishing processing (restriking processing) is performed to the press-formed product 50. According to the restriking processing, when the press-formed product 50 is processed to the shape of a press-formed product 57 shown in
(81) In order to decrease dimension accuracy defects of the press-formed product 57, in general, an advanced estimation of a deformation amount generated by the springback into mold dimensions at the time of design is often performed. However, when the springback is waviness, it is difficult to estimate the deformation amount in advance.
(82) In addition, since correction of the mold in order to solve the waviness of the press-formed product 57 includes trial and error, a lot of time and costs are required for the correction of the mold.
(83) The waviness is generated since the vertical wall portion 55a of the bent portion 52 becomes the extension flange deformation region by the drawing and bending processing (press forming). Accordingly, tensile stress in the longitudinal direction of the press-formed product 50 is increased, and the non-uniformity of the residual stress in the plate thickness direction or the in-plane direction of the press-formed product 50 is promoted.
(84) Due to the non-uniformity of the residual stress of the press-formed product after drawing and bending processing 50, waviness occurs on the press-formed product after restriking processing 57. Accordingly, in order to remove the waviness of the bent portion 52, the wrinkle suppression force applied to the bent portion 52 is preferably increased in the end phase of the press forming of the draw-bending processing.
(85) In order to increase the wrinkle suppression force applied to the bent portion 52 in the end phase of the press forming compared to the straight side portions 51a and 51b, as shown in
(86) As described above, the wrinkle suppression force is increased in the end phase of the press forming, and thus, tension of the vertical wall portion 55a of the bent portion 52, which is the region in which the extension flange deformation occurs, is increased. As a result, the non-uniformity of the residual stress in the plate thickness direction or the in-plane direction, which occurs the springback, of the press-formed product 50 is decreased.
(87) The region in which the shrinkage flange deformation occurs is also similar to the above. That is to say, as described above, the wrinkle suppression force is increased in the end phase of the press forming, and thus, tension of the vertical wall portion 55b of the bent portion 52 which is the region in which the shrinkage flange deformation occurs is also increased. As a result, the springback at the region in which the shrinkage flange deformation occurs is also decreased.
(88) When the pressure receiving portions 30a and 30b are not provided on the wrinkle suppression molds 25a and 25b, the wrinkle suppression molds 25a and 25b are not elastically deformed. The reaction force from the wrinkle suppression force increasing portions 16a and 16b is distributed on the entire wrinkle suppression molds 25a and 25b. Accordingly, the wrinkle suppression force cannot be locally increased on the bent portion 52 in the end phase of the press forming, and thus, the wrinkle suppression force needed in the bent portion 52 cannot be applied.
(89) As a result, tension which is necessary to suppress the springback cannot be applied on the vertical wall portions 55a and 55b of the bent portion 52. Accordingly, effects which is exerted by decreasing the springback of the press-formed product 50 are significantly decreased.
(90) In order to decrease the distribution of the reaction force from the above-described wrinkle suppression force increasing portions 16a and 16b by increasing capability of the wrinkle suppression force increasing portions 16a and 16b, for example, it is necessary to increase the diameter of the disc spring 42a or increase the number of the disc springs 42. In this case, the sizes of the wrinkle suppression force increasing portions 16a and 16b are increased.
(91) On the other hand, in order to press-form a metal plate having a large plastic flow resistance and large springback such as high tensile strength steel or high strength aluminum alloy, since the shape of the press-formed product 50 is curved, it is particularly necessary to increase the wrinkle suppression force in the end phase of the press forming on the region in which the extension flange deformation or the shrinkage flange deformation occurs, or the like.
(92) Accordingly, when the high tensile strength steel, the high strength aluminum alloy, or the like is press-formed, and in the case of decreasing the distribution of the reaction force by increasing the capability of the wrinkle suppression force increasing portions 16a and 16b, it is necessary to significantly increase the sizes of the wrinkle suppression force increasing portions 16a and 16b. Accordingly, it is difficult to dispose the wrinkle suppression force increasing portions 16a and 16b on the press-forming tool 1.
(93) Next, a press-forming tool according to a second embodiment of the present invention will be described.
(94)
(95) A press-forming tool 2 of the present embodiment is the same as the press-forming tool 1 of the first embodiment except that only the wrinkle suppression force increasing portion 16b is provided on the plate 14, the pressure receiving portion 30b formed of a groove portion is disposed only on the wrinkle suppression mold 25b, and a wrinkle suppression mold 25e does not include the pressure receiving portion.
(96) In the press-forming tool 2 according to the present embodiment, the wrinkle suppression force with respect to the blank material 5 can be increased only on the region (only the portion which is particularly added the increased wrinkle suppression force) in which the extension flange deformation occurs. That is to say, when the tensile strength of the blank material 5 is not so high, each of the pressure receiving portion 30b and the wrinkle suppression force increasing portion 16b may be disposed according to curvature or the like of the bent portion 52 of the press-formed product 50.
(97) Next, a press-forming tool according to a third embodiment of the present invention will be described.
(98) A press-forming tool 3 according to the present embodiment is the same as the press-forming tool 1 according to the first embodiment except that wrinkle suppression force increasing portions 16a, 16b, 16c, 16d, 16e, and 16f are disposed on the plate portion 14.
(99) Moreover, the wrinkle suppression molds 25a and 25b of the press-forming tool 3 according to the present embodiment shown in
(100) As shown in
(101) However, compared to the wrinkle suppression force increasing portions 16a and 16b which come into contact with the pressure receiving portions 30a and 30b, in the wrinkle suppression force increasing portions 16c to 16f which come into contact with the first surfaces 31a and 31b not the pressure receiving portions 30a and 30b, the effect which is exerted by increasing the wrinkle suppression force with respect to the blank material 5 is smaller. That is to say, whether or not disposing the wrinkle suppression force increasing portions 16c to 16f which come into contact with the first surface 31a and 31b, which is not the pressure receiving portions 30a and 30b, may be determined according to the shape of the press-formed product or the structure of the press mold.
(102) Next, a press-forming tool according to a fourth embodiment of the present invention will be described.
(103)
(104) A press-forming tool 4 according to the present embodiment is the same as the press-forming tool 1 according to the first embodiment except that the pressure receiving portions 30c and 30d of the wrinkle suppression molds 25c and 25d include groove portions 35c and 35d and the groove portions 35c and 35d, become a portion of the boundary portion and partition the pressure receiving portions 30c and 30d.
(105) In addition, the punch 10 according to the present embodiment shown in
(106) The wrinkle suppression molds 25c and 25d according to the present embodiment are constituted of the minimum number of components which is difficult to divide it further, from the viewpoint of the structure of the press mold and the shape of the press-formed product. That is to say, the wrinkle suppression molds 25c and 25d are not split-type wrinkle suppression molds but integral-type wrinkle suppression molds.
(107) The wrinkle suppression molds 25c and 25d include first surfaces 31c and 31d which oppose the plate portion 14 of the punch 10 and come into contact with the plate portion 14 at the press-forming ending point. In addition, the wrinkle suppression molds 25c and 25d includes second surfaces 32c and 32d which oppose the die 20 and hold the blank material 5 along with the die 20.
(108) In the wrinkle suppression molds 25c and 25d, the pressure receiving portions 30c and 30d which receive the reaction force for elastically deforming the wrinkle suppression molds 25c and 25d in the end phase of the press forming are provided on the first surfaces 31c and 31d. The pressure receiving portions 30c and 30d include the groove portions 35c and 35d. The groove portions 35c and 35d become a portion of the boundary portion, and the pressure receiving portions 30c and 30d are partitioned on the first surfaces 31c and 31d.
(109) Specifically, as shown in
(110) In the end phase of the press forming, the pressure receiving portions 30c and 30d and the wrinkle suppression force increasing portions 16a and 16b come into contact with each other, and thus, the wrinkle suppression molds 25c and 25d are elastically deformed. As a result, it is possible to locally add the wrinkle suppression force to the portion of the blank material 5 which is added the increased wrinkle suppression force.
(111) Accordingly, the wrinkle suppression force in the shrinkage flange deformation region or the extension flange deformation region can be locally increased in the end phase of the press forming, and thus, it is possible to effectively suppress the springback.
(112) In the end phase of the press forming, the wrinkle suppression molds 25c and 25d receive the reaction force from the wrinkle suppression force increasing portions 16a and 16b by the pressure receiving portions 30c and 30d, the wrinkle suppression molds 25c and 25d include the groove portions 35c and 35d. Accordingly, the reaction force is not distributed to the entire wrinkle suppression molds 25c and 25d.
(113) If the wrinkle suppression molds 25c and 25d receive the reaction force from the wrinkle suppression force increasing portions 16a and 16b, the wrinkle suppression molds 25c and 25d are convexly and elastically deformed to the die 20 (blank material 5) side with the groove portions 35c and 35d as the boundary portion. As a result, it is possible to locally and intensively increase the wrinkle suppression force with respect to the blank material 5.
(114) The depths, widths, or the like of the groove portions 35c and 35d of the present embodiment are not particularly limited. The groove portions 35c and 35d may have appropriate dimensions according to the shape of the press-formed product 50 and the structure of the press mold 4. The thickness L of each of the wrinkle suppression mold 25c and 25d in the pressure receiving portions 30c and 30d excluding the groove portions 35c and 35d, and the thickness H of each of the wrinkle suppression mold 25c and 25d in the region which excludes the pressure receiving portions 30c and 30d and comes into contact with the blank material 5 are not particularly limited.
(115) In the present embodiment, although it is shown that the aspect in which the thickness L and the thickness H are the same as each other, it is sufficient that the thickness L is 20LH. Moreover, if the thickness L satisfies 20LH, similar to the first embodiment, it is sufficient that the protruding height G of each of the wrinkle suppression force increasing portions 16a and 16b is 0.02PS+HLG0.3PS+HL.
(116) The press-forming tools 1 to 4 according to the first to fourth embodiments of the present invention are described above. Next, effective positions to dispose the wrinkle suppression force increasing portions 16a to 16f and the pressure receiving portions 30a to 30d will be described.
(117)
(118)
(119) That is to say,
(120) In
(121) As shown in
(122) In this way, in the press-formed product 50 which is press-formed using the press-forming tool 91 of the related art, the plate thicknesses in respective portions in the flange portions 54a and 54b are not the same as one another. The second surfaces 32e and 32f of wrinkle suppression molds 25e and 25f and the die 20 which hold the blank material 5 are flat.
(123) Accordingly, in the wrinkle suppression mold 91 in which the pressure receiving portions 30a to 30d are not provided like the wrinkle suppression molds 25e and 25f, when the plate thickness of each position in the flange portions 54a and 54b is changed during the press forming, a portion to which the wrinkle suppression force is strongly applied and a portion to which the wrinkle suppression force is weakly applied exist.
(124) If the magnitude of the wrinkle suppression force is changed according to the portion during the press forming, a balance in the plastic flow of the blank material 5 during the plastic deformation is lost. As a result, dimension accuracy of the press-formed product 50 after the press forming is decreased.
(125) In order to suppress the decrease in the dimension accuracy of the press-formed product 50 due to the above-described coexistence of the portion to which the wrinkle suppression force is strongly applied and the portion to which the wrinkle suppression force is weakly applied, it is preferable to increase the wrinkle suppression force at the portion at which the plate thickness in the flange portions 54a and 54b is decreased during the press forming, in the end phase of the press forming.
(126) Specifically, the press-forming tool 91 of the related art in which the pressure receiving portions 30a to 30d and the wrinkle suppression force increasing portions 16a to 16f are removed from the press-forming tools 1 to 4 is set as a reference. A region in which the plate thickness becomes the maximum in the flange portions 54a and 54b of the press-formed product 50 is defined as a plate thickness maximum portion, and a region in which the plate thickness is more than 0% and less than or equal to 97% with respect to the plate thickness maximum portion is defined as a plate thickness decreasing portion. In this case, when viewed along the pressing direction, the pressure receiving portions 30a to 30d of the wrinkle suppression molds 25a to 25d are preferably disposed to overlap with a portion of the plate thickness decreasing portion on the blank material 5.
(127) As a result, the wrinkle suppression force at the portion at which the plate thickness in the flange portions 54a and 54b is decreased during the press forming can be preferably increased in the end phase of the press forming. The wrinkle suppression force on the plate thickness decreasing portion, in which the plate thickness is more than 0% and less than or equal to 97% with respect to the plate thickness maximum portion, is preferably increased in the end phase of the press forming, and thus, the springback of the press-formed product 50 can be effectively decreased.
(128)
(129) As shown in
(130) The wrinkle suppression force increasing portion 16b is preferably disposed such that the wrinkle suppression force increasing portion 16b protrudes toward the pressure receiving portions 30b and 30d, and generate the reaction force opposite to the pressing direction when the wrinkle suppression force increasing portion is pressed in the pressing direction, and elastically deform the wrinkle suppression molds 25b and 25d.
(131) As a result, it is possible to preferably increase the wrinkle suppression force of the curved inside portion 6b in which the plate thickness is decreased in the flange portions 54a and 54b during the press forming, in the end phase of the press forming.
(132) In this way, by disposing the pressure receiving portions 30b and 30d and the wrinkle suppression force increasing portions 16b, the wrinkle suppression molds 25b and 25d are convexly and elastically deformed to the blank material 5 side by the pressure receiving portions 30b and 30d in the end phase of the press forming, and thus, it is possible to locally and intensively increase the wrinkle suppression force on the curved inside portion 6b.
(133) The press-forming tools according to each aspect of the present invention described above are summarized as follows.
(134) (1) The press-forming tools 1 to 4 according to each aspect of the present invention include the punch 10 which includes the punch portion 12 and the plate portion 14 configured to transfer a shape to the blank material 5, the die 20 which is paired with the punch 10 and opposes the punch portion 12, and wrinkle suppression molds 25a to 25d.
(135) The wrinkle suppression molds 25a to 25d include the first surfaces 31a to 31d, the second surfaces 32a to 32d, and the side surfaces (third surfaces) 33a and 33b which are continuous between the first surface 31a to 31d and the second surface 32a to 32d and which oppose the punch portion 12. The wrinkle suppression molds 25a to 25d are disposed between the side surfaces (third surfaces) 33a and 33b and the punch portion 12 via a gap.
(136) The first surfaces 31a to 31d oppose the plate portion 14 and come into contact with the plate portion 14 at the press-forming ending point. The second surfaces 32a to 32d oppose the die 20 and hold the blank material 5 along with the die 20.
(137) The press-forming tools 1 to 4 according to each aspect of the present invention include: pressure receiving portions 30a to 30d which include the groove portion, which receives the reaction force to elastically deform the wrinkle suppression molds 25a to 25d in the end phase of the press forming, on the first surfaces 31a to 31d of the wrinkle suppression molds 25a to 25d; and wrinkle suppression force increasing portions 16a and 16b which are disposed on surfaces opposing the first surfaces 31a to 31d of the plate portion 14, protrude toward the pressure receiving portions 30a to 30d, and generate the reaction force in a direction opposite to the pressing direction when the wrinkle suppression force increasing portions are pressed in the pressing direction in the end phase of press forming.
(138) (2) Based on a case where the pressure receiving portions 30a to 30d and the wrinkle suppression force increasing portions 16a and 16b are removed from the press-forming tools 1 to 4, the region in which the plate thickness is maximum in the flange portions 54a and 54b of the press-formed product 50 is defined as the plate thickness maximum portion. The region in which the plate thickness is more than 0% and less than and equal to 97% with respect to the plate thickness maximum portion is defined as the plate thickness decreasing portion. In this case, the pressure receiving portion 30a to 30d may overlap with a portion of the region corresponding to the plate thickness decreasing portion in the blank material 5 when viewed along the pressing direction.
(139) (3) The pressure receiving portions 30a and 30b is constituted of a groove portion, the thickness of each of the wrinkle suppression molds 25a and 25b in the positions of the pressure receiving portions (groove portions) 30a and 30b is defined as L in mm units. The minimum value of the thickness of each of the wrinkle suppression molds 25a and 25b in the position which excludes the pressure receiving portions (groove portions) 30a and 30b and comes into contact with the blank material 5 is defined as H in mm units. In this case, each of the wrinkle suppression molds 25a and 25b may satisfy the following Expressions 1 and 2, and when the protruding height of each of the wrinkle suppression force increasing portions 16a and 16b from the surface of the plate portion 14 is defined as G in mm units and the press stroke distance from the press-forming starting point to the press-forming ending point is defined as PS in mm units, the protruding height G of each of the wrinkle suppression force increasing portions 16a and 16b may satisfy the following Expression 3.
20L0.8H when 40H50(Expression 1)
20L40 when 50<H80(Expression 2)
0.02PS+HLG0.3PS+HL(Expression 3)
(140) (4) A portion of the boundary which partitions the pressure receiving portions 30c and 30d may be the groove portions 35c and 35d. Specifically, the pressure receiving portions 30c and 30d may include the groove portions 35c and 35d, the groove portions 35c and 35d become a portion of the boundary portion, and thus, the pressure receiving portions 30c and 30d may be partitioned on the first surfaces 31c and 31d.
(141) (5) The wrinkle suppression force increasing portions 16a and 16b may include an elastic body which applies the reaction force.
(142) (6) The elastic body may be at least one of the disc spring 42a, a helical spring, and rubber.
(143) Next, a method for manufacturing the press-formed product 50 which is press-formed using the press-forming tools 1 to 4 according to the embodiments of the present invention will be described.
(144) A method for manufacturing the press-formed product 50 according to an aspect of the present invention, including: a step of increasing the wrinkle suppression force with respect to a portion of the blank material 5 during the press forming in the end phase of the press forming from the position at which the press stroke is 2% to 30% to the forming end position using the press-forming tools 1 to 4 according the above-described aspects, and when the forming start position of the press stroke when the blank material 5 is press-formed is defined as 100% and the forming end position of the press stroke is defined as 0%.
(145) According to the method of manufacturing the press-formed product 50, the springback is suppressed, and thus, the press-formed product 50 having high dimension accuracy can be obtained. In the method for manufacturing, if the position of the press stroke which is a starting position of increasing the wrinkle suppression force is less than 2%, the increase in the wrinkle suppression force is not sufficient, and thus, the effect which is exerted by decreasing the springback may be unstable.
(146) On the other hand, if the position of the press stroke which is a starting position of increasing the wrinkle suppression force is more than 30%, the interval of increasing the wrinkle suppression force becomes too long. Accordingly, the difference in the wrinkle suppression force is decreased between the forming starting position of the press stroke and the forming ending position of the press stork.
(147) Therefore, the effect which is exerted by increasing the wrinkle suppression force only in the end phase of the press forming is decreased, and thus, the springback may occur to the contrary. Moreover, in order to further decrease the springback, the position of the press stroke which is a starting position of increasing the wrinkle suppression force is preferably 5% to 15%.
EXAMPLE 1
(148) Effects of the aspects of the present invention will be further described according to Examples. However, conditions of Examples are conditions adopted to confirm feasibility and effects of the present invention, and the present invention is not limited to the conditions. The present invention adopts various conditions if achieving the object of the present invention without departing from the gist of the present invention.
EXAMPLE 1
(149) The blank material 5 was obtained by laser-cutting the high tensile strength steel sheet in a predetermined shape. The blank material 5 was performed drawing and bending processing (press-forming) so that the shape became a hat-shaped cross section. Moreover, after the drawing and bending processing, the blank material was performed finishing processing (restriking processing). Conditions or the like for each process are described below.
(150) The high tensile strength steel sheet having 1.0 mm in the plate thickness and 590 MPa in the tensile strength was used as the material, the high tensile strength steel sheet was laser-cut so that the shape after the finishing processing (restriking processing) became a cross-section width of 60 mm and a height of 80 mm as shown in
(151) The blank material 5 was performed drawing and bending processing (press-forming) to have the shape (hat-shaped cross section) shown in
(152) As the wrinkle suppression force increasing portions 16a to 16f, the disc spring unit which is a combination of disc springs 42a shown in
(153) In the press-forming tool 3 (the press-forming tool 3 according to the third embodiment) shown in
(154) The thicknesses H of the wrinkle suppression molds 25a and 25b on the region which exclude the pressure receiving portions 30a and 30b and come into contact with the blank material 5, the thicknesses L of the wrinkle suppression molds 25a and 25b on the pressure receiving portion 30a and 30b, and the thickness ratio L/H are shown in Table 1.
(155) The load (reaction force) of the wrinkle suppression force increasing portions 16a to 16f applied to the wrinkle suppression molds 25a and 25b are also shown in Table 1. The load is indicated in the total value of the loads of the disc spring unit disposed on the press-forming tools 1 to 3.
(156) For example, the press-forming tool 3 shown in
(157) In Conventional Example No. 14, the press-forming tool 91 shown in
(158) That is to say, the press-forming tool 1 used in the Reference Example 1 was a press-forming tool in which the wrinkle suppression molds 25e and 25f which did not have the pressure receiving portion and the punch 10 which had the wrinkle suppression force increasing portions 16a and 16b were combined.
(159) TABLE-US-00001 TABLE 1 Press stroke position which is added increased Wrinkle suppression wrinkle Pressure force increasing portion Protrusion suppression receiving Load height Thickness Thickness L/H force No. Reference Figure portion Position (kN) G (mm) H (mm) L (mm) (%) (%) Remark 1 FIGS. 1A to 2 16a, 16b 200 9 50 50 100 15 Reference (100 2) Example 2 FIGS. 1A to 2 30a, 30b 16a, 16b 200 14 50 45 90 15 Reference (100 2) Example 3 FIGS. 1A to 2 30a, 30b 16a, 16b 200 19 50 40 80 15 Example (100 2) 4 FIGS. 1A to 2 30a, 30b 16a, 16b 200 24 50 35 70 15 Example (100 2) 5 FIGS. 7A to 8 30b 16b 100 19 50 40 80 15 Example (100 1) 6 FIG. 9A and 9B 30a, 30b 16a, 16b, 16c 600 19 50 40 80 15 Example 16d, 16e, 16f (100 6) 7 FIG. 7A to 8 30b 16b 100 21 40 28 70 15 Example (100 1) 8 FIG. 7A to 8 30b 16b 100 30 70 49 70 15 Reference (100 1) Example 9 FIG. 7A to 8 30b 16b 100 39 70 40 57 15 Example (100 1) 10 FIG. 7A to 8 30b 16b 100 34 60 35 58 15 Example (100 1) 11 FIG. 1A to 2 30a, 30b 16a, 16b 200 35 50 35 70 33 Example (100 2) 12 FIG. 1A to 2 30a, 30b 16a, 16b 200 16.5 50 35 70 2.5 Example (100 2) 13 FIG. 1A to 2 30a, 30b 16a, 16b 200 16.1 50 35 70 1.8 Reference (100 2) Example 14 FIG. 13A and 50 50 100 0 Conventional 13B Example
(160) The drawing and bending processing (press forming) was performed using a press forming apparatus having a capability of 1960 kN (200 tons). Press forming was performed until the height of the press-formed product 50 became 60 mm as shown in
(161) The press forming apparatus used was a general press forming apparatus which did not have a variable die cushion device or the like.
(162) In No. 1 to No. 10 in the Examples of the present invention and the Reference Examples, the increase in the wrinkle suppression force in the end phase of the press forming started from the height of 9 mm before the press-forming ending point. That is to say, the protruding height G of each of the wrinkle suppression force increasing portions 16a and 16b coming into contact with the pressure receiving portions 30a and 30b in the end phase of the press forming was set to the value which added 9 mm to the depth (H-L) of each of the pressure receiving portions 30a and 30b.
(163) The press stroke distance PS from the press-forming starting point to the press-forming ending point was 60 mm. That is to say, when the forming start position of the press stroke was defined as 100% and the forming end position of the press stroke was defined as 0% during the press-forming of the blank materials, the position of the press stroke which is a starting position of increasing the wrinkle suppression force was positioned at the position of 15%.
(164) Here, the wrinkle suppression force increasing portions 16a and 16b coming into contact with the pressure receiving portions 30a and 30b in the end phase of the press forming is described. However, in the wrinkle suppression force increasing portions 16c to 16f which did not come into contact with the pressure receiving portions 30a and 30b in the end phase of the press forming, the protruding height G was set to 9 mm.
(165) In No. 11 to No. 13 in the Examples of the present invention and the Reference Examples, the increase in the wrinkle suppression force in the end phase of the press forming was controlled as follows. That is to say, as shown in Table 1, the starting position of increasing the wrinkle suppression force was controlled by setting the depth (H-L) of each of the pressure receiving portions 30a and 30b to be constant and changing the value of the protruding height G.
(166) In Example No. 11 of the present invention, the increase in the wrinkle suppression force started from the height (the position in which the press stroke is 33%) of 20 mm before the press-forming ending point. In Example No. 12 of the present invention, the increase in the wrinkle suppression force started from the height (the position in which the press stroke is 2.5%) of 1.5 mm before the press-forming ending point. In Example No. 13 of the present invention, the increase in the wrinkle suppression force started from the height (the position in which the press stroke is 1.8%) of 1.1 mm before the press-forming ending point.
(167) The finishing processing (restriking processing) was performed using the press-formed product 50 obtained by the above-described drawing and bending processing (press forming).
(168)
(169)
(170) In the press-formed product 50 obtained by the drawing and bending processing (press forming), a hat portion surrounded by the vertical wall portions 55a and 55b and the top portion 55c was fitted into the punch portion 12 of the restriking processing mold 92, and the top portion 55c was pressed by a pad 18. The finishing processing (restriking processing) was performed by the punch portion 12 and the die 20. In the finishing processing (restriking processing), the wrinkle suppression was not performed.
(171) The finishing processing (restriking processing) was performed using a press-forming apparatus having a capability of 1960 kN (200 tons). As shown in
(172) The press-forming apparatus used was a general press-forming apparatus which did not include the variable die cushion device or the like.
(173) Next, an evaluation method of the springback with respect to the press-formed product 50 after the drawing and bending processing and the press-formed product after the finishing processing (restriking processing) 57 will be described.
(174)
(175) Specifically, as shown in
(176) W.sub.h, W.sub.h, and W.sub.h may be obtained as follows. Coordinate values of a point group on the outer surface of the press-formed product 50 after the drawing and bending processing are acquired using a non-contact type CCD three-dimensional measurement apparatus. In the cross-sectional view when viewed from the arrow A direction in
(177) Based on W.sub.h obtained in the above-described way, the wall warpage (springback) after the drawing and bending processing (press forming) was evaluated according to the following reference.
(178) Good (G): W.sub.h is less than or equal to 10 mm
(179) Not Bad (NB): W.sub.h is more than 10 mm and less than 15 mm
(180) Bad (B): W.sub.h is equal to or more than 15 mm
(181)
(182) Specifically, as shown in
(183) W.sub.c, W.sub.c, and W.sub.c may be obtained as follows. Coordinate values of a point group on the outer surface of the press-formed product after the finishing processing (restriking processing) 57 are acquired using a non-contact type CCD three-dimensional measurement apparatus. In the cross-sectional view when viewed from the arrow B direction in
(184) Based on W.sub.c obtained in the above-described way, the wall warpage (springback) after the finishing processing (restriking processing) was performed was evaluated according to the following reference.
(185) Good (G): W.sub.c is less than or equal to 7 mm
(186) Not Bad (NB): W.sub.c is more than 7 mm and less than 15 mm
(187) Bad (B): W.sub.c is equal to or more than 15 mm
(188) Moreover,
(189)
(190)
(191) The waviness 61 of the press-formed product 57 may be evaluated as follows. Coordinate values of a point group on the outer surface of the press-formed product after the finishing processing (restriking processing) 57 are acquired using a non-contact type CCD three-dimensional measurement apparatus. The measured results of the coordinate values in the line segment 62 in the curved face 60 are compared with the CAD data (design shape) when the press-formed product 57 is designed, and thus, the graph shown in
(192) An absolute value Y.sub.W of the difference between the maximum value and the minimum value in the graph in the curved face 60 is obtained as shown in
(193) Based on Y.sub.w obtained in this way, the waviness 61 (springback) after the finishing processing (restriking processing) was evaluated according to the following reference.
(194) Very Good (VG): Y.sub.w is less than or equal to 3 mm
(195) Good (G): Y.sub.w is more than 3 mm and less than 7 mm
(196) Not Bad (NB): Y.sub.w is more than 7 mm and less than 15 mm
(197) Bad (B): Y.sub.w is equal to or more than 15 mm
(198) Evaluation results of the springback with respect to the press-formed product 50 after the drawing and bending processing and the press-formed product 57 after the finishing processing (restriking processing) are shown in Table 2. After performing the drawing and bending processing and the restriking processing, cracks were not confirmed in the press-formed product 50 or the press-formed product 57 under any conditions.
(199) TABLE-US-00002 TABLE 2 Springback Crack Wh Wc Yw No. Occurrence (mm) Evaluation (mm) Evaluation (mm) Evaluation Remark 1 None 16 B 13 NB 14 NB Reference Example 2 None 13 NB 10 NB 8 NB Reference Example 3 None 7 G 5 G 5 G Example 4 None 6 G 4 G 4 G Example 5 None 10 G 7 G 7 G Example 6 None 9 G 7 G 7 G Example 7 None 5 G 5 G 5 G Example 8 None 10 NB 9 NB 8 NB Reference Example 9 None 5 G 4 G 4 G Example 10 None 5 G 3 G 3 VG Example 11 None 8 G 6 G 5 G Example 12 None 9 G 7 G 5 G Example 13 None 18 B 14 NB 16 B Reference Example 14 None 21 B 15 B 18 B Conventional Example
(200) First, the evaluation result of the springback with respect to the press-formed product 50 after the drawing and bending processing is described. As shown in Table 2, in any one of the Examples No. 3 to No. 7 and No. 9 to No. 12 of the present invention, it was confirmed that W.sub.h after the drawing-bending processing was performed was good and the wall warpage (springback) was small.
(201) On the other hand, in any one of Reference Examples No. 1, No. 2, No. 8, and No. 13, and Conventional Example No. 14, W.sub.h, after the drawing and bending processing was performed was not better than W.sub.h of the Example of the present invention.
(202) By comparing the Examples No. 3 and No. 6 of the present invention, when only the wrinkle suppression force increasing portions 16a and 16b were disposed, it was confirmed that the effect which is exerted by decreasing the springback was higher than when the wrinkle suppression force increasing portions 16a to 16f were disposed. That is to say, when only the wrinkle suppression force increasing portions 16a and 16b were disposed, the wrinkle suppression molds 25a and 25b were remarkably bent in the end phase of the press forming, compared to when the wrinkle suppression force increasing portions 16c to 16f are disposed.
(203) As a result, it could be confirmed that the springback in the press-formed product 50 could be further decreased.
(204) By comparing No. 1 to No. 4 in the Examples of the present invention and the Reference Examples, it could be confirmed that the thickness H and the thickness L preferably satisfy the above-described Expressions 1 and 2. In No. 1 to No. 4, only the thickness L of each of the wrinkle suppression molds 25a and 25b was changed, and other press-forming conditions were the same as one another.
(205) In No. 1 to No. 4, the values of the protruding heights G were different from one another. However, above all, the position of the press stroke which is a starting position of increasing the wrinkle suppression force was 15% in these Examples, which was the same as one another.
(206) Among No. 1 to No. 4, the thickness L exceeded 0.8H in No. 1 and No. 2, and the thickness L was less than or equal to 0.8H in No. 3 and No. 4. That is to say, in No. 3 and No. 4 which were examples satisfying Expression 1 or 2 in No. 1 to No. 4, the springback could be preferably decreased.
(207) Here,
(208)
(209) In
(210) As shown in
(211) Accordingly, the portion which is particularly added the increased wrinkle suppression force on the flange portions 54a and 54b and a portion of the region (the region on which the pressure receiving portions 30a and 30b are provided) in which the contact pressure is preferably increased on the second surfaces 32a and 32b overlap with each other when viewed along the pressing direction.
(212) By comparing No. 4, No. 11 to No. 13 which are the Examples of the present invention and the Reference Examples, it could be confirmed that the protruding height G of each of the wrinkle suppression force increasing portions 16a and 16b preferably satisfy the above-described Expression 3. In No. 4, No. 11 to No. 13, only the position of the press stroke which is a starting position of increasing the wrinkle suppression force is changed by changing the value of the protruding height G, and other press forming conditions are the same as one other.
(213) Among No. 4, No. 11 to No. 13, in No. 11, the position of the press stroke which is a starting position of increasing the wrinkle suppression force is 33%. In No. 13, the position of the press stroke which is a starting position of increasing the wrinkle suppression force is 1.8%.
(214) On the other hand, among No. 4, No. 11 to No. 13, in No. 4, the position of the press stroke which is a starting position of increasing the wrinkle suppression force is 15%. In No. 12, the position of the press stroke which is a starting position of increasing the wrinkle suppression force is 2.5%.
(215) That is to say, among No. 4, No. 11 to No. 13, the protruding height G satisfies Expression 3 in No. 4 and No. 12. In this way, in No. 4 and No. 12 which are the examples satisfying Expression 3 among No. 4, No. 11 to No. 13, it could be confirmed that the springback could be preferably decreased.
(216) On the other hand, as described above, in Reference Example No. 1 and No. 2, since the thickness L exceeded 0.8H, the springback could not be decreased. In Reference Example No. 8, since the thickness L exceeded 40 mm, the springback could not be decreased.
(217) As described above, in Reference Example No. 13, since the position of the press stroke which is a starting position of increasing the wrinkle suppression force was 1.8% and the increase of the wrinkle suppression force in the end phase of the press forming was not sufficient, the springback could not be decreased. In Conventional Example No. 14, since the pressure receiving portions 30a and 30b and the wrinkle suppression force increasing portions 16a and 16b were not provided, the springback could not be decreased.
(218) Next, the evaluation method of the springback with respect to the press-formed product after the finishing processing (restriking processing) 57 will be described. As shown in Table 2, in any one of the Examples No. 3 to No. 7 of the present invention, it could be confirmed that No. 9 to No. 12, W.sub.c and Y.sub.w after the finishing processing (restriking processing) were good and the wall warpage and the waviness 61 were small.
(219) It could be confirmed that the dimension accuracy of the press-formed product after the finishing processing (restriking processing) 57 was improved as the springback of the press-formed product after the drawing and bending processing 50 was decreased. This is because the tensile stress in the longitudinal direction of the press-formed product 50 on the vertical wall surfaces 55a and 55b of the bent portion 52 is decreased by increasing the wrinkle suppression force of the bent portion 52 in the end phase of the press forming in the drawing and bending processing.
(220) As a result, the non-uniformity of the residual stress in the plate thickness direction or the in-plane direction of the press-formed product 50 is decreased, and thus, the dimension accuracy of the press-formed product after the finishing processing (restriking processing) 57 is also improved.
(221) On the other hand, in any one of Reference Examples No. 1, No. 2, No, 8, and No. 13 and Conventional Example No. 14, W.sub.c and Y.sub.w after the restriking processing were not better than W.sub.c and Y.sub.w of the Example of the present invention. In this way, if the springback of the press-formed product after the drawing and bending processing 50 was large, even when the finishing processing (restriking processing) was performed, it could be confirmed that the dimension accuracy of the press-formed product 57 was not improved.
EXAMPLE 2
(222)
(223) Specifically, a high tensile strength steel sheet having 1.0 mm in the plate thickness and 590 MPa in the tensile strength was used as the material, and similar to the Example 1, the high tensile strength steel sheet was laser-cut, and thus, the blank material 5 was obtained. The blank material 5 was performed the drawing and bending processing (press forming) to have the shape (hat-shaped cross section) shown in
(224) Table 3 shows combinations of the disposed positions of the pressure receiving portions 30a, 30b, and 30g to 30j and the wrinkle suppression force increasing portions 16a to 16f. For example, the press-forming tool of Example No. 16 of the present invention is the same as the press-forming tool 2 of Example No. 5 of the present invention of the Example 1 except for the thickness H, the thickness L, and the thickness ratio L/H.
(225) The load (reaction force) applied to the wrinkle suppression molds 25a and 25b by the disc spring unit of the wrinkle suppression force increasing portions 16a to 16f was set to 150 kN. Moreover, the protruding height G was set to 19 mm. The press stroke distance PS from the press-forming starting point to the press-forming ending point was set to 60 mm. That is to say, when the forming start position of the press stroke was set to 100% and the forming end position of the press stroke was set to 0% during the press-forming of the blank material 5, the position of the press stroke which is a starting position of increasing the wrinkle suppression force was set to 6.7%.
(226) After the drawing and bending processing, the finishing processing (restriking processing) was performed. The conditions of the drawing and bending processing, the conditions of the restriking processing, and the evaluation method of the springback were similar to those of the Example 1.
(227) TABLE-US-00003 TABLE 3 Press Stroke Position which is added increased Wrinkle suppression wrinkle Pressure force increasing portion Protrusion suppression Reference receiving Load height Thickness Thickness L/H force No. figure portion Position (kN) G (mm) H (mm) L (mm) (%) (%) Remark 15 FIG. 26 30a 16a 150 19 50 35 70 6.7 Reference (150 1) Example 16 FIG. 26 30b 16b 150 19 50 35 70 6.7 Example (150 1) 17 FIG. 26 30g 16c 150 19 50 35 70 6.7 Reference (150 1) Example 18 FIG. 26 30h 16d 150 19 50 35 70 6.7 Reference (150 1) Example 19 FIG. 26 30i 16e 150 19 50 35 70 6.7 Reference (150 1) Example 20 FIG. 26 30j 16f 150 19 50 35 70 6.7 Reference (150 1) Example
(228) The evaluation results of the springback with respect to the press-formed product after the drawing and bending processing 50 and the press-formed product after the finishing processing (restriking processing) 57 are shown in Table 4. After the drawing and bending processing and the restriking processing were performed, in any condition, cracks were not confirmed in the press-formed product 50 or the press-formed product 57.
(229) TABLE-US-00004 TABLE 4 Springback Crack Wh Wc Yw No. Occurrence (mm) Evaluation (mm) Evaluation (mm) Evaluation Remark 15 None 12 NB 10 NB 10 NB Reference Example 16 None 7 G 6 G 6 G Example 17 None 18 B 14 NB 15 B Reference Example 18 None 15 B 12 NB 13 NB Reference Example 19 None 19 B 14 NB 15 B Reference Example 20 None 15 B 12 NB 14 NB Reference Example
(230) As shown in Table 4, in Example No. 16 of the present invention, W.sub.h after the drawing and bending processing, and W.sub.c and Y.sub.w after the finishing processing were good, and it could be confirmed that the springback was small.
(231) In Example No. 16 of the present invention, the pressure receiving portion 30b was disposed so that the pressure receiving portion overlapped with a portion of the curved inside portion 6b which becomes the plate thickness decreasing portion having the plate thickness more than 0% and less than or equal to 97% with respect to the curved outside portion 6a which becomes the plate thickness maximum portion on the flange portion 54a and 54b of the press-formed product 50 press-formed by the press-forming tool 91 of the related art.
(232) That is to say, in Example No. 16 of the present invention, the wrinkle suppression force could be locally and intensively increased to the curved inside portion 6b which is necessary to increase the wrinkle suppression force in the end phase of the press forming, which was difficult to be achieved by the press-forming tool 91 of the related art.
(233) On the other hand, in any one of Reference Example No. 15 and No. 17 to No. 20, W.sub.h, W.sub.c, and Y.sub.w were not better than Example No. 16 of the present invention. As shown in Table 4, in Reference Example No. 15 and No. 17 to No. 20, the pressure receiving portions 30a and 30g to 30j were disposed so that the pressure receiving portions overlapped with not the curved inside portion 6b which becomes the plate thickness decreasing portion but at least a portion of the curved outside portion 6a or the straight line portions 6c to 6f.
(234) Accordingly, the wrinkle suppression force could not be increased to the curved inside portion 6b which is necessary to increase the wrinkle suppression force in the end phase of the press forming. In general, in the press-formed product 57, it is required that the dimensions on the entire region of the press-formed product 57 are within a permitted range.
(235) That is to say, the press-formed product 57 in which the dimensions are outside the permitted range even at one site, for example, the press-formed products 57 of the Reference Examples No. 15 and Nos. 17 to 20 are not preferable.
(236) As described above, if the wrinkle suppression force on the plate thickness decreasing portion which is necessary to increase the wrinkle suppression force was increased in the end phase of the press forming, it could be confirmed that the dimension accuracy of the press-formed product after the drawing and bending processing 50 and the press-formed product after the finishing processing (restriking processing) 57 could be preferably improved.
INDUSTRIAL APPLICABILITY
(237) As described above, according to an aspect of the present invention, a pressure receiving portion is provided on a portion of a wrinkle suppression mold, and a wrinkle suppression force increasing portion is provided on a portion of a punch. The pressure receiving portion and the wrinkle suppression force increasing portion come into contact with each other in the end phase of the press forming, and thus, the wrinkle suppression mold is elastically deformed.
(238) As a result, the wrinkle suppression force generated from the wrinkle suppression force increasing portion is sufficiently transmitted to the portion of a blank material which is added the increased wrinkle suppression force in the end phase of press forming.
(239) That is to say, even when the press-formed product includes an extension flange deformation region in addition to a shrinkage flange deformation region, springback of the press-formed product can be effectively decreased. Accordingly, the industrial applicability thereof is high.
BRIEF DESCRIPTION OF THE REFERENCE SYMBOLS
(240) 1 to 4: press-forming tool
(241) 5: blank material
(242) 6a: curved outside portion (plate thickness maximum portion)
(243) 6b: curved inside portion (plate thickness decreasing portion)
(244) 6c to 6f: straight line portion
(245) 10: punch
(246) 12: punch portion
(247) 14: plate portion
(248) 16a to 16f: wrinkle suppression force increasing portion (disc spring unit)
(249) 20: die
(250) 25a to 25f: wrinkle suppression mold
(251) 30a, 30b, and 30g to 30j: pressure receiving portion (groove portion)
(252) 30c and 30d: pressure receiving portion
(253) 31a to 31f: first surface
(254) 32a to 32f: second surface
(255) 33a and 33b: third surface (side surface)
(256) 35c and 35d: groove portion
(257) 40a: pin
(258) 42a: disc spring (elastic body)
(259) 50: press-formed product after drawing and bending processing
(260) 51a and 51b: straight side portion
(261) 52: bent portion
(262) 54a, 54a, 54b, and 54b: flange portion
(263) 55a, 55a, 55b, and 55b: vertical wall portion
(264) 55c: top portion
(265) 57: press-formed product after the finishing processing (restriking processing)
(266) 60: curved face
(267) 61: waviness
(268) 62: line segment
(269) G: protruding height
(270) H and L: thickness