Abstract
There is provided a method of manufacturing a metal shell formed body by cold forging for a metal shell of a spark plug. In the manufacturing method, a semi-finished formed body is first provided with a second inner step without the formation of an annular front end portion. After the semi-finished formed body is inserted from its front end side into a die, a punch is pushed into the semi-finished formed body from its rear end side. By pushing the punch, an annular front-facing surface of the punch is pushed onto the second inner step so as to press a front end portion of the formed body against an annular front end portion forming part of the die. By such a forming step, the metal shell formed body is obtained in which the annular front end portion is formed by extrusion.
Claims
1. A method of manufacturing a metal shell formed body for a spark plug, the metal shell formed body comprising: a body part having formed therein an axial hole for insertion of an insulator and having formed thereon a radially outwardly protruding flanged portion; a cylindrical intermediate portion located in front of the body part; and an annular front end portion located in front of the cylindrical intermediate portion and made smaller in outer diameter than the cylindrical intermediate portion, the manufacturing method comprising the steps of: a semi-finished formed body producing step for cold forging a metal material, to produce a semi-finished formed body with the flanged portion and the cylindrical intermediate portion, the flanged portion having a front facing surface, the semi-finished formed body having an axial hole faulted therein along a center axis thereof such that the axial hole includes, in order of mention from the rear to the front, a large-diameter hole region, a first middle-diameter hole region smaller in diameter than the large-diameter hole region, a small-diameter hole region smaller in diameter than the first middle-diameter hole region and a second middle-diameter hole region larger in diameter than the small-diameter hole region; and an annular front end portion forming step for, after the semi-finished formed body producing step, forming the annular front end portion by pushing a punch into the semi-finished formed body and thereby pressing a front end portion of the semi-finished formed body against a die while maintaining said front-facing surface of the flanged portion spaced from contact with the die.
2. The manufacturing method of the metal shell formed body for the spark plug according to claim 1, wherein the semi-finished formed body producing step includes forming a first inner step between the large-diameter hole region and the first middle-diameter hole region and forming a second inner step between the first middle-diameter hole region and the small-diameter hole region; and wherein the die is fittable around the semi-finished formed body by clearance fitting and having an inner circumferential cylindrical surface shaped to mate with the cylindrical intermediate portion, a reduced-diameter inner cylindrical surface smaller in inner diameter than the inner circumferential cylindrical surface and a tapered inner circumferential surface between the inner circumferential cylindrical surface and the reduced-diameter inner cylindrical surface; wherein the punch has an annular front-facing surface shaped to push at least one of the first and second inner steps; wherein the annular front end portion forming step includes: inserting and placing the semi-finished formed body from a front end side thereof into the die; and pushing the punch into the semi-finished formed body from a rear end side thereof so as to, by pushing of the annular front-facing surface onto at least one of the first and second inner steps, force the semi-finished formed body toward the front, press a front end portion of the semi-finished formed body against the reduced-diameter inner cylindrical surface and the tapered inner circumferential surface of the die and thereby form the annular front end portion by cold forging.
3. The manufacturing method of the metal shell formed body for the spark plug according to claim 2, wherein the punch is shaped to push both of the first and second inner steps and force the semi-finished formed body toward the front.
4. The manufacturing method of the metal shell formed body for the spark plug according to claim 3, wherein an axial dimension of the small-diameter hole region of the semi-finished formed body is larger than a design dimension of a small-diameter hole region of the metal shell formed body; and wherein an axial dimension from the first inner step to the second inner step of the semi-finished formed body is smaller than a design dimension between first and second inner steps of the metal shell formed body.
5. The manufacturing method of the metal shell formed body for the spark plug according to claim 1, wherein the semi-finished formed body producing step includes forming a first inner step between the large-diameter hole region and the first middle-diameter hold region; and wherein the manufacturing methods further comprises, after the semi-finished formed body producing step and before or in parallel with the annular front end portion forming step, a step for forming a second inner step between the first middle-diameter hole region and the small-diameter hole region.
6. The manufacturing method of the metal shell formed body for the spark plug according to claim 5, wherein the semi-finished formed body producing step includes forming a temporary tapered portion between the first middle-diameter hole region and the small-diameter hole region; and wherein the die is fittable around the semi-finished formed body by clearance fitting and having an inner circumferential cylindrical surface shaped to mate with the cylindrical intermediate portion, a reduced-diameter inner cylindrical surface smaller in inner diameter than the inner circumferential cylindrical surface and a tapered inner circumferential surface between the inner circumferential cylindrical surface and the reduced-diameter inner cylindrical surface; wherein the punch has an annular front-facing surface shaped to push the first inner step and a small-diameter hold region forming surface shaped to push the temporary tapered portion; wherein the annular front end portion forming step includes: inserting and placing the semi-finished formed body from a front end side thereof into the die; and pushing the punch into the semi-finished formed body from a rear end side thereof so as to, by at least one of pushing of the annular front-facing surface onto the first inner step and pushing of the small-diameter hole region forming surface onto the temporary tapered portion, force the semi-finished formed body toward the front, press a front end portion of the semi-finished formed body against the reduced-diameter inner cylindrical surface and the tapered inner circumferential surface of the die and thereby form the annular front end portion by cold forging and, at the same time, press the small-diameter hole region forming surface of the punch against the temporary tapered portion of the semi-finished formed body and thereby form the second inner step by cold forging.
7. The manufacturing method of the metal shell formed body for the spark plug according to claim 5, wherein an axial dimension of the small-diameter hole region of the semi-finished formed body is larger than a design dimension of a small-diameter hole region of the metal shell formed body; and wherein an axial dimension from the first inner step to the second inner step of the semi-finished formed body is smaller than a design dimension between first and second inner steps of the metal shell formed body.
8. A manufacturing method of a metal shell for a spark plug, further comprising: manufacturing the metal shell formed body by the manufacturing method according to claim 1; and forming a thread on at least a part of the cylindrical intermediate portion of the metal shell formed body.
9. A manufacturing method of a spark plug, comprising: manufacturing a metal shell by the manufacturing method according to claim 8; and placing an insulator in the metal shell formed body.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1) FIG. 1 shows cross sections of formed bodies (A-F) in respective steps of cold forging process for formation of a metal shell formed body from a starting raw material according to one embodiment of the present invention.
(2) FIG. 2 schematically shows the first step for formation of the semi-finished formed body (A) of FIG. 1 by the use of a die, where the left side is a section view of the formed body before extrusion; and the right side is a section view of the formed body after extrusion.
(3) FIG. 3 schematically shows the second step for formation of the semi-finished formed body (B) of FIG. 1 by the use of a die, where the left side is a section view of the formed body before extrusion; and the right side is a section view of the formed body after extrusion.
(4) FIG. 4 schematically shows the third step for formation of the semi-finished formed body (C) of FIG. 1 by the use of a die, where the left side is a section view of the formed body before extrusion; and the right side is a section view of the formed body after extrusion.
(5) FIG. 5 schematically shows the fourth step for formation of the semi-finished formed body (D) of FIG. 1 by the use of a die, where the left side is a section view of the formed body before extrusion; and the right side is a section view of the formed body after extrusion.
(6) FIG. 6 schematically shows the fifth step for formation of the semi-finished formed body (E) of FIG. 1 by the use of a die, where the left side is a section view of the formed body before extrusion; and the right side is a section view of the formed body after extrusion.
(7) FIG. 7 schematically shows the sixth step (final forming step) for formation of the metal shell formed body (F) of FIG. 1 with the annular front end portion by the use of a die, where the left side (left illustration) is a section view of the formed body before extrusion; and the right side (right illustration) is a section view of the formed body after extrusion.
(8) FIG. 8 shows one example of the sixth step (final forming step) for formation of the annular front end portion by pressing a first inner step of the semi-finished formed body (E) with an annular front-facing surface of a punch while holding the formed body in the die, where the left side (left illustration) is a section view of the formed body before extrusion; and the right side (right illustration) is a section view of the formed body after extrusion.
(9) FIG. 9 shows another example of the sixth step (final forming step) for formation of the annular front end portion by pushing first and second inner steps of the semi-finished formed body (E) with a punch while holding the formed body in the die, where the left side (left illustration) is a section view of the formed body before extrusion; and the right side (right illustration) is a section view of the formed body after extrusion.
(10) FIG. 10 shows a state where the axial dimension L2 of a small-diameter hole region of the semi-finished formed body (E) is larger than a design dimension L2f of the metal shell formed body (F); and the axial dimension L3 from the second inner step to the first inner step in the small-diameter hole region of the semi-finished formed body (E) is smaller than a design dimension L3f of the metal shell formed body (F).
(11) FIG. 11 shows a cross section of a conventional type of spark plug.
(12) FIG. 12 shows a cross section of a metal shell before being assembled into the spark plug of FIG. 11.
(13) FIG. 13 shows, half in section, a metal shell formed body before being subjected to cutting for manufacturing of the metal shell of FIG. 12.
(14) FIG. 14 shows of formed bodies (semi-finished products) in respective steps of cold forging process for formation of the metal shell formed body of FIG. 13 from a starting raw material.
(15) FIG. 15 shows cross sections of dies used in the first to fifth steps for formation of the metal shell formed body of FIG. 13.
(16) FIG. 16 schematically shows a comparison of metal shell formed bodies having the same thread diameter and thread length (length of cylindrical intermediate portion) but different axial positions of second inner steps.
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
(17) A manufacturing method (cold forging method) of a metal shell formed body for a spark plug according to one embodiment (first embodiment) of the present invention will be described below with reference to FIGS. 1 to 7. As the metal shell formed body 30f manufactured in the present embodiment is substantially the same as that shown in FIG. 13, an explanation of the metal shell formed body itself will be omitted herefrom. FIG. 1 shows a series of six process steps A to F for forming (manufacturing) the metal shell formed body 30f in the present embodiment. The respective process steps (first to sixth steps) until the completion of the metal shell formed body 30 (sixth-step formed product) in the sixth step (final forging step; as corresponding to the claimed annular front end portion forming step) will be explained one by one with reference to FIG. 1. FIGS. 2 to 6 respectively show the first to fifth steps (as corresponding to the claimed semi-finished formed body producing step). In each of FIGS. 2 to 6, the left side of the center line (vertical center line) is a half section of the raw material (semi-finished formed body) before the corresponding step; and the right side of the center line (vertical center line) is a half section of the formed body (formed product) after the corresponding step. In the respective cross sections of FIGS. 2 to 7, cross hatching of any dies other than upper and lower main dies (such as die and punch) are omitted as appropriate. In FIGS. 1 to 7, the parts and portions of the formed body corresponding to those of the metal shell (or metal shell formed body) in FIGS. 12 and 13 are principally designated by the same reference numerals.
(18) The details of the respective process steps are as follows. In the present embodiment, the raw material (cylindrical column-shaped material) is sequentially subjected to forming as shown in FIG. 1. Through the cold forging operations from the first to fifth steps (semi-finished formed body producing step) as shown in FIGS. 2 to 6, the raw material is formed into a semi-finished formed body 30e (fifth-step formed product) (see the illustration E of FIG. 1) before the final forming step for completion of the metal shell formed body. The semi-finished formed body 30e is in a state before the formation of the annular front end portion 32 in front of the cylindrical intermediate portion 35 to be threaded. Then, the semi-finished formed body 30e is inserted and placed into a die (lower die) as shown in the left side of FIG. 7, followed by pushing a punch 240f into the semi-finished formed body 30e from its upper end side as shown in the right side of FIG. 7. In such an annular front end portion forming step, the semi-finished formed body 30f (sixth-step formed product) is obtained in which the annular front end portion 32 is formed in front of the cylindrical intermediate portion 35 to be threaded (see the illustration F of FIG. 1). The die (lower die) 200f used in this sixth step is fitted around the semi-finished formed body by clearance fitting and has a circular hole formed with an inner circumferential cylindrical surface 203f so as to mate with a cylindrical part (circular cylindrical part) 35e of the semi-finished formed body 30e, which is to be processed into the cylindrical intermediate portion 35 and the annular front end portion 32 of the metal shell formed body 30f, with substantially no clearance left therebetween, and a circular hole located coaxially at a lower end of the above-mentioned circular hole and formed with a reduced-diameter inner cylindrical surface 206f so as to shape the outer circumferential surface of the annular front end portion 32. There is a tapered inner circumferential surface (rear-facing annular surface) 205f tapered down between the inner circumferential cylindrical surface 203f and the reduced-diameter inner cylindrical surface 206f in the die 200f. An inner diameter of the reduced-diameter inner cylindrical surface 206f is set equal to an outer diameter of the annular front end portion 32.
(19) Namely, the semi-finished formed body 30e (fifth-step formed product 30e) having the cylindrical part 35e, which is to be processed into the cylindrical intermediate portion 35 and the annular front end portion 32 of the metal shell formed body 30f, is formed as shown in the illustration E of FIG. 1 before the formation of the metal shell formed body 30f as shown in the illustration F of FIG. 1. The semi-finished formed body 30e is inserted and placed from its front end side into the die (lower die) 200f (see the left side of FIG. 7). As mentioned above, the die 200f is fitted around the semi-finished formed body by clearance fitting and has the inner circumferential cylindrical surface 203f shaped to mate with the cylindrical part 35e, the tapered inner circumferential surface 205f and the reduced-diameter inner cylindrical surface 206f as an annular front end portion forming surface whose inner diameter is reduced to be equal to the outer diameter of the annular front end portion 32. Then, the punch (upper die) 240f is pushed into the semi-finished formed body 30e from its rear end side (upper side) (see the left side of FIG. 7). The punch 240f has an annular front-facing surface 243f shaped to push the second inner step 44 of the semi-finished formed body 30e. By pushing the punch, the annular front-facing surface 243f of the punch is pushed onto the second inner step 44 of the semi-finished formed body 30e so as to force the semi-finished formed body 30e toward the front (front end side) and press a front end portion (lower end portion in FIG. 7) of the cylindrical part 35e of the semi-finished formed body 30e against the tapered inner circumferential surface 205f and the reduced-diameter inner cylindrical surface 206f as the annular front end portion forming surface of the die. In this pushing, the annular front end portion 32 is formed by extrusion (see the enlarged area in the right side of FIG. 7) in front of the cylindrical intermediate portion 35. There is thus completed the metal shell formed body 30f as shown in the illustration F of FIG. 1. Hereinafter, the first to fifth steps as the semi-finished formed body producing step (cold forging step) and the sixth step as the annular front end portion forming step) will be respectively explained in detail below.
(20) First Step
(21) As shown in FIG. 2, the first step is performed by the use of a lower die (die) 200a having a different-diameter circular hole (hollow hole) with a large-diameter upper hole region 203a and a small-diameter lower hole region. The cylindrical column-shaped starting raw material S, which has been cut out according to the size of the finished product, is inserted and placed into the circular hole region 203a of the die from above (see the left side of the vertical center line (center line) in FIG. 2). Herein, an inner diameter of the small-diameter lower circular hole region 205a is set slightly smaller than the outer diameter of the cylindrical intermediate portion 35 of the metal shell formed body 30f of FIG. 13; and an inner diameter of the large-diameter upper circular hole region 203a is set substantially equal to the outer diameter of the annular cylindrical crimp portion 38 of the metal shell formed body 30f of FIG. 13. After the insertion and placement of the raw material, a cylindrical column-shaped supporting punch (pin) 220a and a sleeve 240a are inserted into the small-diameter circular hole region 205a of the die from below. A circular shaft-shaped punch 250a is pushed into the raw material S from above such that the raw material S is compressed between an end face of the punch 250a and end faces of the punch 220a and the sleeve 240a. Thus, a first-step formed product (different-diameter cylindrical column-shaped formed body) 30a is obtained (see FIG. 1-A and FIG. 2). The first-step formed product 30a has a large-diameter rear part 39a and a small-diameter part 35a, with a tapered portion provided therebetween, as shown in the right side of the center line in FIG. 2. Further, recesses are formed in the centers of both front and rear end faces of the first-step formed product 30a. After the completion of the above forming operation, the first-step formed product 30a is discharged out by pulling out the punch 250a and knocking out the supporting punch 220a in synchronism with the punch 250a. In the respective process steps, the coaxial vertical movement of the die, the driving (vertical movement) of the supporting punch and the knock-out pin (knock-out sleeve) for support of the raw material (semi-finished formed body) and the discharging of the formed body are known techniques. An explanation of these techniques will be omitted hereinafter.
(22) Second Step
(23) As explained below with reference to FIG. 3, the second step is performed by the use of a die 200b assembled from first and second lower die components 201b and 202b. The first lower die component 201b has a circular hole 203b shaped to restrain an outer circumferential surface of the small-diameter part 35a of the first-step formed product 30a, whereas the second lower die component 202b is located above the first lower die component 201b and has a circular hole coaxial with the circular hole 203b. The circular hole 207b of the second lower die component 202b has an inner circumferential surface substantially equal in diameter to the outer circular circumferential surface of the flange 36 of the metal shell formed body 30f of FIG. 13. A cylindrical column-shaped supporting pin 220b and a cylindrical sleeve 270b are inserted into the circular hole 203b of the die 200b from below.
(24) A hole punch 240b is arranged at an upper side of the die (lower die) 200b coaxially (concentrically) with the circular holes 203b and 207b. This hole punch 240b is designed to form a bottomed circular hole in the rear end face of the large-diameter part 39a of the first-step formed product 30a and thereby shape the inner circumferential surface of the large-diameter body part 39 such as thin annular crimp portion 38 and flange 36 of the metal shell formed body 30f. Consequently, the hole punch 240b is circular in section; and an outer diameter of the hole punch 240b is set substantially equal to the inner diameter of the inner circumferential surface 48 of the body part 39 of the metal shell formed body 30f, i.e., the inner diameter of the large-diameter hole region 48a. However, a front end part of the hole punch 240b is made relatively small in diameter such that the hole punch 240b is formed into a different-diameter shape for pre-forming of the first inner step 46 on the middle region of the inner circumferential surface of the metal shell formed body 30f.
(25) An extrusion sleeve (cylindrical tube) 250b, which has a larger inner diameter than the outer diameter of the hole punch 240b, is coaxially fitted around the hole punch 240b through a spacer (cylindrical tube) 260b. By the spacer (cylindrical tube) 260b, a front end part of the extrusion sleeve 250b is maintained at a predetermined space (cylindrical clearance) apart from the hole punch 240 throughout its circumference. As the thin annular crimp portion 38 is formed by extrusion in the space (cylindrical clearance), the space (cylindrical clearance) is maintained in front of the spacer (cylindrical tube) 260b at all times in the present invention. An inner circumferential surface of the extrusion sleeve 250b is circular in shape. An inner diameter of the extrusion sleeve 250b is set slightly smaller than the outer diameter of the large-diameter part 39a of the first-step formed product 30a and substantially equal to the outer diameter of the thin annular crimp portion 38 of the metal shell formed body 30f of FIG. 13. An outer circumferential surface of the extrusion sleeve 250b is circular in shape such that the extrusion sleeve 250b is fittable in the circular hole 207b of the die 200b by clearance fitting. The extrusion sleeve 250b is vertically movable in synchronism with or separately from the hole punch 240b so as to extrude the thin annular crimp portion 38 toward the rear between the front end region of the inner circumferential surface of the extrusion sleeve 250b and the outer circumferential surface of the hole punch 240b.
(26) In the second step, the small-diameter part 35a of the first-step formed product 30a is inserted and placed in the circular hole 203b of the die 200b as shown in the left side of the center line in FIG. 3. After the insertion and placement of the formed body, the cylindrical column-shaped supporting pin 220b and the sleeve 270b are inserted into the circular hole 203b from below; and the hole punch 240b and the extrusion sleeve 250b are inserted into the circular hole 203b from above. The first-step formed product 30a is compressed between these dies 220b, 270b and 240b, 250b. More specifically, the extrusion sleeve 250 is pushed down as appropriate so as to engage an upper end portion of the large-diameter part 39a of the first-step formed product 30a. Then, the hole punch 240b is pushed into a rear end face of the large-diameter part 39a of the first-step formed body 30a by a predetermined stroke. By such pushing, the bottomed hole is formed, with a predetermined depth and a diameter substantially equal to the inner diameter of the inner circumferential surface 48 (large-diameter hole region 48a) of the body part 39, in the rear end face of the large-diameter part 39a of the first-step formed body 30a as shown in the right side of the center line in FIG. 3. At this time, the first inner step 46 is pre-formed. At the completion of the above pushing operation, the thin annular crimp portion 38 is formed by extrusion between the front end region of the inner circumferential surface of the extrusion sleeve 250b and the outer circumferential surface of the hole punch 240b (see the right side of the center line in FIG. 3). Thus, a second-step formed product 30b having at its rear end the thin annular crimp portion 38 is obtained (see FIG. 1-B).
(27) Third Step
(28) As explained below with reference to FIG. 4, the third step is performed to elongate the cylindrical part (small-diameter part 35a and large-diameter part 39a) of the second-step formed product 30b. In the third step, dies such as lower die and hole punch are used as shown in FIG. 4. The die (lower die) 200c assembled from first and second lower die components 201c and 202c. The first lower die component 201c has a circular hole 203c shaped to restrain the outer circumferential surface of the small-diameter part 35a of the second-step formed product 30b, whereas the second lower die component 202c is located above the first lower die component 201c and has a circular hole 207c formed coaxial with the circular hole 203c and shaped to restrain the outer circumferential surface of the large-diameter part 39a of the second-step formed product 30b. As in the case of the second step, a cylindrical column-shaped supporting pin 220c and a cylindrical sleeve 270c are inserted into the circular hole 203c of the die 200c from below. The die 200c is thus similar in structure to that used in the second step although the height (axial length) of the second lower die component 202c is set larger than that in the second step.
(29) A deep hole punch 240c is arranged at an upper side of the die (lower die) 200c coaxially (concentrically) with the circular holes 203c and 207c. This deep hole punch 240c is adapted to perform deep perforation to perforate the large-diameter hole region 48a of the large-diameter part 39a of the second-step formed product 30b toward the front relative to the first inner step 46 and thereby form the first middle-diameter hole region 41a as corresponding to the inner circumferential surface 41 of the cylindrical intermediate portion 35 of the metal shell formed body and, at the same time, elongate (extrude toward the front) the small-diameter part 35a and thereby form the cylindrical intermediate portion 35. As the body part 39 of the metal shell formed body 30f and the first middle-diameter hole region 41a of the cylindrical intermediate portion 35 are shaped by the hole punch 240c, the hole punch 240c has a front end part substantially equal in diameter to the inner diameter of the cylindrical intermediate portion 35 and a rear part set substantially equal in diameter to the inner diameter of the body part 39, with a press surface (annular stepped surface) being defined therebetween for formation of the first inner step 46. A small-diameter portion is provided on a front end of the hole punch 240c. As shown in the left side of the center line in FIG. 4, the second-step formed product 30b is inserted and placed in the circular holes 203c and 207c. The deep hole punch 240c is then pushed down into the bottom of the hollow rear end region of the second-step formed product 30b by a predetermined stroke, thereby compressing the second-step formed product 30b between an end face of the hole punch 240c and an end face of the cylindrical column-shaped supporting pin 220c while extruding the small-diameter part toward the front to form a cylindrical portion 35c to be processed into the cylindrical intermediate portion 35. At this time, the body part 39 is extruded and elongated toward the rear. Thus, a third-step formed product 30c is obtained (see FIG. 1-C). Herein, the pushing stroke of the deep hole punch 240c is set in such a manner as to leave a bottom wall K of predetermined thickness on a region of the inner circumferential surface 41 of the cylindrical portion 35c corresponding to the small-diameter hole region 43a of the metal shell formed body.
(30) Fourth Step
(31) As will be explained below with reference to FIG. 5, the fourth step is performed to form the polygonal portion 37 on the outer circumferential surface of the body part 39 of the third-step formed product 30c. In the fourth step, a die (lower die) with a cylindrical support member 200d and a cylindrical column member 210d is used as shown in FIG. 5. The cylindrical support member 200d has a circular hole 203d shaped to hold therein the cylindrical portion 35c of the third-step formed product 30c with a slight clearance left therebetween and a supporting rear end surface 205d shaped to, when the cylindrical portion 35 is inserted in the circular hole 203d, support thereon an annular front-facing surface of the third-step formed product 30 formed in rear of the cylindrical portion 35c. The cylindrical column member 210d is arranged on an inner circumference of the cylindrical support member 200d so as to support a front end (lower end) of the cylindrical portion 35c by an upper end (tip end) of the cylindrical column member 210d.
(32) Also used is an upper die assembled from an inner circumferential surface supporting die component 240d and a polygonal portion forming die component 220d. The inner circumferential surface supporting die component 240d has a cylindrical column shape formed with a different-diameter front end so as to, when the inner circumferential surface supporting die component 240d is inserted into the third-step formed product 30c from its rear end side, allow a clearance left between the front end of the inner circumferential surface supporting die component 240d and the bottom wall K but substantially no clearance between the inner circumferential surface supporting die component 240d and the inner circumferential surface 48 of the third-step formed product 30c. The polygonal portion forming die component 220d is arranged coaxially with the inner circumferential surface supporting die component 240d and has an inner circumferential surface (polygonal portion forming surface) shaped to form the polygonal portion 37 on the outer circumferential surface of the body part 39 of the third-step formed product 30c by being pushed from above. The inner circumferential surface of the polygonal portion forming die component 220d includes a front region formed into a circular shape so as to surround the large-diameter part of the third-step formed product 30c with substantially no clearance left therebetween and a rear region formed over a predetermined range and, when viewed in section, having its inner circumference 223d in agreement with the outer profile of the polygonal portion 37 of the metal shell formed body 30f. The polygonal portion forming die component 220d is coaxially disposed around the inner circumferential surface supporting die 240 via a collar sleeve 250d so as not to cause interference of the polygonal portion forming die component 220d with the thin annular crimp portion 38 during this forming operation.
(33) The third-step formed product 30c is inserted from its cylindrical portion 35 into the cylindrical support member (lower die) 200d. The inner circumferential surface supporting die component (upper die) 240d is pushed down by a predetermined stroke. In such a state, the polygonal portion forming die component 220d is pushed down by a predetermined stroke. By this, a given axial region of the outer circumferential surface of the body part 39 of the third-step formed product 30 is extruded and formed as the polygonal portion 39. Thus, a fourth-step formed product 30d is obtained (see FIG. 1-D).
(34) Fifth Step
(35) As shown in FIG. 6, the fifth step is performed to punch out the remaining bottom wall K of the deep hole of the fourth-step formed product 30d by the use of a stamping punch. A die 200e is also used, having a circular hole 203e shaped to mate with the cylindrical portion 35d of the fourth-step formed product. Further, a cylindrical column member 200e is coaxially arranged in the circular hole of the die so as to support a front end of the cylindrical portion 35d. As shown in the left side of FIG. 6, the cylindrical portion 35d of the fourth-step formed product 30d is inserted and placed in the circular hole 203e. In such a state, the bottom wall K is punched out from above by the cylindrical stamping punch 240e as shown in the right side of FIG. 6. Thus, a fifth-step formed product 30e with an axial through hole is obtained (see FIG. 1-E). In this punching operation, the small-diameter hole region 43a is formed with the inner circumferential surface 43 by shearing of the bottom wall K. The inner circumferential region of the formed body located in front of the small-diameter hole region 43a is defined as the second middle-diameter hole region 41b smaller in diameter than the small-diameter hole region 43a. The inner circumferential surface 43 of the small-diameter hole region 43 is consequently shaped as an annular inward protrusion, thereby forming not only the second inner step 44 between the first middle-diameter hole region 41a and the small-diameter hole region 43a but also an annular front-facing step 45 between the small-diameter hole region 43a and the second middle-diameter hole region 41b. By the above punching operation, there is obtained the fifth-step formed product 30e (as corresponding to the semi-finished formed body) having formed thereon the cylindrical part 35e to be processed into the cylindrical intermediate portion 35. The metal shell formed body 30f is obtained by forming the annular front end portion 32 on the fifth-step formed product 30e in the subsequent step (sixth step).
(36) Sixth Step
(37) The sixth step (final cold forging step) is performed with the use of the die as shown in FIG. 7. The lower die 200f is assembled from two vertically aligned die components 201f and 202f. As mentioned above, the first lower die component 201f has a circular hole formed with the inner circumferential cylindrical surface 203f and the reduced-diameter inner cylindrical surface 206f such that the cylindrical part 35e of the fifth-step formed product 30e is fittable in the circular hole by clearance fitting. The inner circumferential cylindrical surface 203f is shaped to mate with the cylindrical part 35e of the fifth-step formed product 30e. The reduced-diameter inner cylindrical surface 206f is located below and coaxially with the inner circumferential cylindrical surface 203f and is formed with a reduced inner diameter equal to the outer diameter of the annular front end portion 32 so as to shape the outer circumferential surface of the annular front end portion 32. The tapered inner circumferential surface 205f is formed between the inner circumferential cylindrical surface 203f and the reduced-diameter inner cylindrical surface 206f and tapered down toward the front. Herein, the annular front end portion forming surface is constituted by the inner circumferential cylindrical surface 203f, the tapered inner circumferential surface 205f and the reduced-diameter inner cylindrical surface 206f. A cylindrical column member 220f is coaxially inserted from below in the circular hole of the first lower die component 201f. This die is shaped to be fitted in the second middle-diameter hole region 41b, which is located in front of the small-diameter hole region 43a on the inner circumferential surface 41 of the cylindrical part 35e, with no clearance left therebetween, and thereby restrain the inner circumferential surface of the second middle-diameter hole region 43a by its outer circumferential surface and, at the same time, allow contact between its upper end and the front-facing step 45 of the small-diameter hole region 43a. Further, a sleeve 270f is arranged around the cylindrical column member 220f so as to kick out the formed product after the extrusion of the annular front end portion 32 in the sixth step. The second lower die component 202f is located on an upper surface 210f of the first lower die component 201f and has a circular hole 207 formed coaxial with the circular hole of the inner circumferential cylindrical surface 203f so as to receive therein the flange 36 of the fifth-step formed product 30e by clearance fitting.
(38) The punch (annular front end portion forming punch) 240f is arranged at an upper side of the lower die 200f coaxially with the circular hole 207f. The annular front-facing surface 243f of the punch 240f is shaped to, when the punch 240f is inserted in the fifth-step formed product (semi-finished formed body) 30e from its rear end side, push the second inner step 44 of the small-diameter hole region 43a. The punch 240f has a front end part (lower end part) 244f located in front of the annular front-facing surface 243f and formed with a small outer diameter so as to be fitted in the small-diameter hole region 43a and a circular shaft part 245f located in rear of the front end part and formed with an outer diameter so as to be fitted in the first middle-diameter hole region 41a of the cylindrical part 35e with substantially no clearance left therebetween.
(39) In the sixth step, the semi-finished formed body 30e is inserted and placed in the die so that the cylindrical part 35e of the semi-finished formed body 30e is fitted in and mates with the inner circumferential cylindrical surface 203f of the first lower die component 201f as shown in the left side of FIG. 7. The punch (annular front end portion forming punch) 240f is pushed into the semi-finished formed body 30e so as to push the annular front-facing surface 243f onto the second inner step 44 of the small-diameter hole region 43a (see the enlarged area in the right side of FIG. 7). Then, the semi-finished formed body 30e is forced toward the front such that the outer circumferential surface of the front end portion of the cylindrical part 35e is pressed against the annular front end portion forming surface such as tapered inner circumferential surface 205f of the die (first lower die component 2010 as shown in the right side of FIG. 7 (see, in particular, the middle enlarged area of FIG. 7). By the above pushing operation, the annular front end portion 32 is extruded toward the front (lower side of FIG. 7). The semi-finished formed body 30e is thus processed into the metal shell formed body 30f. Namely, the metal shell formed body 30f in which the annular front end portion 32 is formed in front of the cylindrical middle portion 35 (see the enlarged area in FIG. 1-F) is obtained as desired as shown in FIG. 16 through the cold forging process.
(40) As the axial length of the annular front end portion 32 varies depending on the pushing amount (stroke) of the punch (annular front end portion forming punch) 240f, it is feasible to set the pushing amount of the punch 240f according to the desired axial length of the annular front end portion 32. In the pushing operation, the stroke of the punch 240f may be set by locking a front end of the punch 240f on a tip end of the cylindrical column member 220f in the circular hole of the lower die component 201f. In other words, the punch 240f and the lower die 200f may be so structured as to, when the annular front end portion 32 is formed by pushing the punch 240f and pressing the front end portion of the cylindrical part 35e toward the front, bring the lower end of the punch 240f into contact with the tip end of the cylindrical column member 220f inside the lower die 200f.
(41) As described above, the annular front end portion 32 is formed in front of the cylindrical intermediate portion 35 in the final step of the cold forging process for manufacturing of the metal shell formed body in the present embodiment. This enables manufacturing of the metal shell formed bodies by forming the annular front end portions 32 with the use of one kind of die (first lower die component 201f) in the step for completion of the metal shell formed bodies, as long as the annular front end portions 32 are the same in shape and dimension, even in the case where the metal shells differ in the axial position of the second inner step 44 or slightly differ in the length of the thread 34 although the threads 34 formed on the outer circumferential surfaces of the cylindrical intermediate portions 35 are the same in diameter. It is therefore possible to significantly reduce the number of dies, as compared to that in the conventional manufacturing method, for cost reduction of the metal shell formed body 30f. As also obvious from FIG. 7, the above process can be applied even in the case where the metal shells slightly differ in the length of the thread. The reason for this is that there is a clearance S left between the front-facing surface of the flange 36 and the upper surface of the first lower die component 201f (see the right side of FIG. 7) during the formation of the metal shell formed body 30f with the annular front end portion 32.
(42) The thus-obtained metal shell formed body 30f, or the metal shell cut body obtained by cutting of the metal shell formed body 30f, is completed as a metal shell 30 by welding the ground electrode to the front end of the formed body and forming (by e.g. rolling) the thread on at least part of the outer circumferential surface of the cylindrical intermediate portion of the formed body. There is obtained a spark plug 1 by placing an insulator with a center electrode etc. into the metal shell 30. The use of such a metal shell 30 allows a reduction in the cost of the spark plug.
(43) In the above embodiment, the punch (annular front end portion forming punch) 240f is pushed into the semi-finished formed body 30e from its rear end side so as to push the annular front-facing surface 243 of the punch 240f onto the second inner step 44 of the semi-finished formed body 30e, force the semi-finished formed body 30e toward the front and thereby press the front end portion of the cylindrical part 35e against the tapered inner circumferential surface 205f of the die component 201f. The annular front end portion 32 is formed by such pushing operation in the above embodiment. In the present invention, however, the part of the semi-finished formed body 30e pushed by the punch is not limited to the second inner step 44 as mentioned above. For example, it is feasible to form the annular front end portion 32 in the sixth step (final forming step) by the use of a punch having an annular front-facing surface shaped to push the first inner step 46 of the semi-finished formed body 30e. This alternative embodiment will be explained later in detail. Further, the annular front end portion 32 is formed in the annular front end portion forming step subsequent to the formation of the semi-finished formed body 30e in which the second inner step 44 is provided between the first middle-diameter hole region 41a and the small-diameter hole region 43a in the above embodiment. In the present invention, however, the step for forming the second inner step 44 between the first middle-diameter hole region 41a and the small-diameter hole region 43a and the step for forming the annular front end portion 32 may be performed after the formation of the semi-finished formed body.
(44) Hereinafter, the embodiment in which the first inner step 46 of the semi-finished formed body 30e is pushed in the sixth step will be explained with reference to FIG. 8. This embodiment is different from the above embodiment, only in the configuration of the punch (annular front end portion forming punch) 240f pushed into the semi-finished formed body 30e in the step of FIG. 7. Thus, the same parts and portions (corresponding parts and portions) are designated by the same reference numerals as those in FIG. 7; and only the differences in configuration will be explained below. In this embodiment, the punch (annular front end portion forming punch) 240f has a circular shaft part 247f shaped so as to, when the punch 240f is pushed into the semi-finished formed body 30e from the rear, be inserted by clearance fitting in the large-diameter hole region 48a of the body part 39 of the semi-finished formed body 30e as shown in the left side of FIG. 8. The punch 240f also has a circular shaft part 245f formed coaxially in front of the circular shaft part 247f and made smaller in diameter than the circular shaft part 247f so as to be fitted in the first middle-diameter hole region 41a of the cylindrical part 35e by clearance fitting. There is an annular front-facing surface 246f defined on a boundary between these circular shaft parts 245f and 247f so as to push the first inner step 46 of the semi-finished formed body 30e. As shown in FIG. 8, the annular front-facing surface 246f is concave curved in shape corresponding to the convex curved cross-sectional profile of the first inner step 46.
(45) Accordingly, the punch (annular front end portion forming punch) 240f is pushed into the semi-finished formed body 30e from the rear as shown in the right side of FIG. 8 in this embodiment. Then, the annular front-facing surface 246f of the punch 240 is pushed onto the front inner step 46 of the semi-finished formed body 30e so as to force the semi-finished formed body 30e toward the front as shown in the enlarged area of the FIG. 8. In such pushing, the annular front end portion 32 is formed by pressing the front end region of the outer circumferential surface of the cylindrical part 35e against the tapered inner circumferential surface 205f and the reduced-diameter inner cylindrical surface 206f of the die component 201f as in the case of FIG. 7. As the first inner step 46 is larger in inner diameter than the second inner step 44, it is possible in this embodiment ensure not only a pushing position radially closer to the annular front end portion 32 when axially viewed (from the rear) but also a large pushing area for stable pushing.
(46) In another alternative embodiment of FIG. 9, the punch (annular front end portion forming punch) 240f may be formed corresponding to the combination of the punches of FIGS. 7 and 8 so as to push both of the second inner step 44 and the first inner step 46 of the semi-finished formed body (E) by two front and rear annular front-facing surfaces 243f and 246f (see the enlarged area of FIG. 9). In this alternative embodiment, the punch 240f has a small-diameter front end part (lower end part) 244f shaped to be fitted in the small-diameter hole region 43a, a circular shaft part 245f shaped to be fitted in the first middle-diameter hole region 41a of the cylindrical intermediate portion 35, with substantially no clearance left therebetween, and a circular shaft part 247f shaped to be fitted by clearance fitting in the large-diameter hole region 48a of the body part 39 (see the left side of FIG. 9). These parts 244f, 245f and 247 are arranged coaxially in the order from the front such that the punch 240f becomes larger in diameter toward the rear. The annular front-facing surface 243f is formed on a boundary between the front end part (lower end part) 244f and the circular shaft part 245f so as to push the second inner step 44. The annular front-facing surface 246f is formed into a concave curved shape on a boundary between the circular shaft part 245f and the circular shaft part 247f so as to push the first inner step 46. By the use of such a punch 240f, it is possible to ensure a larger pushing area for more stable pushing.
(47) In the case of using the punch of FIG. 9, the forming operation is performed as follows. The punch (annular front end portion forming punch) 240f is first pushed into the semi-finished formed body 30e so as to simultaneously allow pushing of the annular front-facing surface 243f onto the second inner step 44 of the small-diameter hole region 43a and pushing of the annular front-facing surface 246f onto the first inner step 46 (see the enlarged area of FIG. 9). Then, the semi-finished formed body 30e is forced toward the front such that the outer circumferential surface of the front end portion of the cylindrical part 35e is pressed against the annular front end portion forming surface such as tapered inner circumferential surface 205f of the die (first lower die component 2010. By the above pushing operation, the annular front end portion 32 is extruded toward the front. The semi-finished formed body 30e is thus processed into the metal shell formed body 30f. Namely, the metal shell formed body 30f in which the annular front end portion 32 is formed in front of the cylindrical middle portion 35 (see the enlarged area in FIG. 1-F) is obtained as desired as shown in FIG. 16 through the cold forging process. In the punch (annular front end portion forming punch) 240f of FIG. 9, the axial dimensions of the two front and rear annular front-facing surfaces 243f and 246f are set as appropriate according to the axial dimension of the second inner step 44 of the small-diameter hole region 43a and the axial dimension of the first inner step 46 of the metal shell finished body, respectively.
(48) Alternatively, the second inner step 44 at the rear end of the small-diameter hole region 43 of the semi-finished formed body 30e may be a tapered portion reduced in diameter toward the front and temporarily provided during the forming operation (in an unfinished state), i.e., a temporary tapered portion (temporary second inner step; hereinafter referred to as temporary tapered portion) as shown in the left section view of FIG. 10. In this case, the annular front-facing surface 243f of the punch 240f of FIG. 9 serves as a small-diameter hole region forming surface to push the temporary tapered portion 44 and shape the small-diameter hole region 43a with the temporary tapered portion 44 to a design dimension during the formation of the annular front end portion 32. For the formation of the annular front end portion 32, the punch 240f is pushed into the semi-finished formed body 30e from the rear so as to push the temporary tapered portion 44, i.e., the unfinished second inner step by the annular front-facing surface 243f, i.e., the small-diameter hole region forming surface and force the semi-finished formed body 30e toward the front. By such pushing, the annular front end portion 32 is cold forged by pressing the front end portion of the semi-finished formed body 30e against the reduced-diameter inner cylindrical surface 206f and the tapered inner circumferential surface 205f of the die. Simultaneously, the second inner step 44 is cold forged by pressing the small-diameter hole region forming surface against the temporary tapered portion.
(49) In the case of pushing both of the second inner step 44 and the first inner step 46 of the semi-finished formed body 30e, it is preferable to perform the forming operation as follows. An axial dimension L2 of the small-diameter hole region 43a of the semi-finished formed body 30e as shown in the left section view of FIG. 10 is set larger than a design dimension L2f of the small-diameter hole region 43 of the metal shell formed body 30f as shown in the right section view of FIG. 10; and an axial dimension L3 from the second inner step 44 of the small-diameter hole region 43a to the first inner step 45 of the semi-finished formed body 30e as shown in the left section view of FIG. 10 is set smaller than a design dimension L3f between the inner steps 44 and 46 of the metal shell formed body 30f as shown in the right section view of FIG. 10. Then, the annular front end portion 32 is extruded toward the front such that both of the dimensions L2 and L3 are simultaneously adjusted to the respective design dimensions L2f and L3f. In other words, the axial dimension (design dimension) L3f from the second inner step 44 to the first inner step 46 is attained during the extrusion forming of the annular front end portion 32 in the cold forging process. It is possible by such forming operation to improve the accuracy of the axial dimension. Herein, the outer circumferential surface of the small-diameter front end part (lower end part) of the punch 240f fitted in the small-diameter hole region 43a as shown in FIG. 9 serves to shape the inner circumferential surface of the small-diameter hole region 43a. Further, the cylindrical column member 220f is inserted in the second middle-diameter hole region 41b from below so as to restrain the front-facing step 45 of the small-diameter hole region 43a.
(50) In the present invention, the shape of the metal shell formed body is not limited to those of the above embodiments. The axial lengths of the cylindrical intermediate portion, the annular front end portion and the small-diameter hole region and the axial positions of the first and second inner steps can be set as appropriate. Further, it is possible in the present invention to manufacture the metal shell formed bodies by sharing the annular front end portion forming die in the cold forging step, even though the cylindrical intermediate portions slightly differ in length from one another, as long as the cylindrical intermediate portions are the same in outer diameter and the annular front end portions are the same in outer diameter. In all of the process steps (FIGS. 2-9) of the present invention, the respective formed bodies (A to F) of FIG. 1 are formed by cold forging. The punching of the fifth step (FIG. 6) is also included in the cold forging.
DESCRIPTION OF REFERENCE NUMERALS
(51) 1: Spark plug 21: Insulator of spark plug 30: Metal shell of spark plug 30f: Metal shell formed body 30e: Semi-finished formed body 32: Annular front end portion 34: Thread (screw thread) 35: Cylindrical intermediate portion 39: Body part 41: Inner circumferential surface of cylindrical intermediate portion 41a: First middle-diameter hole region 41b: Second middle-diameter hole region 43: Inner circumferential surface of small-diameter hole region 43a: Small-diameter hole region 44: Second inner step 46: First inner step 48a: Large-diameter hole region 200f: Die in which semi-finished formed body is inserted 201f: Die having annular front end portion forming portion in which semi-finished body is inserted 203f: Inner circumferential cylindrical surface of die in which semi-finished formed body is inserted 205f: Tapered inner circumferential surface of die in which semi-finished body is inserted 206f: Reduced-diameter inner cylindrical surface of die in which semi-finished body is inserted 240f: Punch (annular front end portion forming punch) 243f, 246f: Annular front-facing surface