Apparatus and method for dynamic control of plated uniformity with the use of remote electric current
09567685 ยท 2017-02-14
Assignee
Inventors
- Burhanuddin Kagajwala (Hillsboro, OR, US)
- Bryan L. Buckalew (Tualatin, OR, US)
- Steven T. Mayer (Lake Oswego, OR)
- Lee Peng Chua (Beaverton, OR)
- Aaron Berke (Portland, OR)
- James Isaac Fortner (Newberg, OR, US)
- Robert Rash (West Linn, OR)
Cpc classification
C25D17/001
CHEMISTRY; METALLURGY
C25D17/06
CHEMISTRY; METALLURGY
C25D7/123
CHEMISTRY; METALLURGY
C25D17/002
CHEMISTRY; METALLURGY
C25D17/10
CHEMISTRY; METALLURGY
International classification
C25D17/00
CHEMISTRY; METALLURGY
C25D17/10
CHEMISTRY; METALLURGY
C25D17/06
CHEMISTRY; METALLURGY
Abstract
An apparatus for electroplating metal on a substrate while controlling plating uniformity includes in one aspect: a plating chamber having anolyte and catholyte compartments separated by a membrane; a primary anode positioned in the anolyte compartment; an ionically resistive ionically permeable element positioned between the membrane and a substrate in the catholyte compartment; and a secondary electrode configured to donate and/or divert plating current to and/or from the substrate, wherein the secondary electrode is positioned such that the donated and/or diverted plating current does not cross the membrane separating the anolyte and catholyte compartments, but passes through the ionically resistive ionically permeable element. In some embodiments the secondary electrode is an azimuthally symmetrical anode (e.g., a ring positioned in a separate compartment around the periphery of the plating chamber) that can be dynamically controlled during electroplating.
Claims
1. An electroplating apparatus for electroplating a metal on a substrate, the apparatus comprising: (a) a plating chamber configured to contain an electrolyte, the plating chamber comprising a catholyte compartment and an anolyte compartment, wherein the anolyte compartment and the catholyte compartment are separated by an ion-permeable membrane; (b) a substrate holder configured to hold and rotate the substrate in the catholyte compartment during electroplating; (c) a primary anode positioned in the anolyte compartment of the plating chamber; (d) an ionically resistive ionically permeable element positioned between the ion-permeable membrane and the substrate holder, wherein the ionically resistive ionically permeable element is adapted to provide ionic transport through the element during electroplating; and (e) a secondary anode configured to donate plating current to the substrate, wherein the secondary anode is positioned such that the donated plating current does not cross the ion-permeable membrane separating the anolyte and catholyte compartments, and wherein the secondary anode is positioned such as to donate plating current through the ionically resistive ionically permeable element, wherein the ionically resistive ionically permeable element comprises at least three portions: (i) an outer, ionically permeable portion; (ii) a middle, ionically impermeable portion; and (iii) an inner, ionically permeable portion, wherein the apparatus is configured to donate plating current from the secondary anode through the outer, ionically permeable portion, but not through the inner ionically permeable portion.
2. The apparatus of claim 1, wherein the secondary anode is an azimuthally symmetrical anode.
3. The electroplating apparatus of claim 2, wherein the primary anode has a diameter or width that is smaller than a diameter or width of a plating face of the substrate.
4. The electroplating apparatus of claim 2, wherein a portion of the plating chamber housing the primary anode has a diameter or width that is smaller than a diameter or width of a plating face of the substrate.
5. The apparatus of claim 2, wherein the secondary anode is positioned in a secondary anode compartment, around the periphery of the plating chamber.
6. The apparatus of claim 2, wherein the secondary anode compartment is separated from the catholyte compartment by an ion-permeable membrane.
7. The apparatus of claim 2, wherein the secondary anode is a consumable anode.
8. The apparatus of claim 2, wherein the secondary anode is a consumable anode comprising copper.
9. The apparatus of claim 2, wherein the secondary anode is an inert anode.
10. The apparatus of claim 2, wherein the ionically resistive ionically permeable element is separated from a plating surface of the substrate by a gap of 10 mm or less.
11. The apparatus of claim 10, further comprising an inlet to the gap for introducing electrolyte flowing to the gap and an outlet to the gap for receiving electrolyte flowing through the gap, wherein the inlet and the outlet are positioned proximate azimuthally opposing perimeter locations of a plating face of the substrate, and wherein the inlet and outlet are adapted to generate cross-flow of electrolyte in the gap.
12. The apparatus of claim 2, wherein the secondary anode is positioned in a secondary anode compartment, and wherein the apparatus comprises one or more channels for irrigating the secondary anode in the secondary anode compartment.
13. The apparatus of claim 2, wherein the secondary anode is positioned in a secondary anode compartment, and wherein the apparatus comprises one or more channels for collecting and removing bubbles from the secondary anode compartment.
14. The apparatus of claim 2, wherein the ionically resistive ionically permeable element is azimuthally asymmetric and comprises an azimuthally asymmetrically positioned portion that does not allow the plating current to pass through the ionically resistive ionically permeable element.
15. The apparatus of claim 1, wherein the middle, ionically impermeable portion of the ionically resistive ionically permeable element has a smaller surface on a side of the ionically resistive ionically permeable element that is closest to the substrate than on the opposite side of the element.
16. The apparatus of claim 1, wherein the apparatus is configured to dynamically control the secondary anode during electroplating.
17. A method of electroplating a metal on a cathodically biased substrate, the method comprising: (a) providing the substrate into an electroplating apparatus configured for rotating the substrate during electroplating, wherein the apparatus comprises: (i) a plating chamber configured to contain an electrolyte, the plating chamber comprising a catholyte compartment and an anolyte compartment, wherein the anolyte compartment and the catholyte compartment are separated by an ion-permeable membrane; (ii) a substrate holder configured to hold and rotate the substrate in the catholyte compartment during electroplating; (iii) a primary anode positioned in the anolyte compartment of the plating chamber; (iv) an ionically resistive ionically permeable element positioned between the ion-permeable membrane and the substrate holder, wherein the ionically resistive ionically permeable element is adapted to provide ionic transport through the element during electroplating and wherein the ionically resistive ionically permeable element comprises at least three portions: an outer, ionically permeable portion; a middle, ionically impermeable portion; and an inner, ionically permeable portion; and (v) a secondary anode configured to donate plating current to the substrate, wherein the secondary anode is positioned such that the donated plating current does not cross the ion-permeable membrane separating the anolyte and catholyte compartments and wherein the secondary anode is positioned such as to donate plating current through the ionically resistive ionically permeable element; (b) electroplating the metal on the substrate while rotating the substrate, and while providing power to the secondary anode and the primary anode, wherein the donated plating current from the secondary anode passes through the outer, ionically permeable portion of the ionically resistive ionically permeable element, but not through the inner ionically permeable portion.
18. The method of claim 17, further comprising: (c) after electroplating metal on the substrate, electroplating metal on a second substrate that has a different distribution of recessed features in an outer portion of the second substrate than the substrate, without substituting any mechanical shields in the apparatus.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1)
(2)
(3)
(4)
(5)
(6)
(7)
(8)
(9)
(10)
(11)
(12)
(13)
(14)
DETAILED DESCRIPTION
(15) Methods and apparatus for electroplating a metal on a substrate while controlling uniformity of the electroplated layer, such as radial uniformity, azimuthal uniformity, or both, are provided. The methods are particularly useful for sequentially electroplating metal on dissimilar substrates, such as on semiconductor wafers having different patterns or distribution of recessed features on the surface. The methods control plating current (ionic current) at the substrate using a remotely positioned secondary electrode.
(16) Embodiments are described generally where the substrate is a semiconductor wafer; however the invention is not so limited. Provided apparatus and methods are useful for electroplating metals in TSV and WLP applications, but can also be used in a variety of other electroplating processes, including deposition of copper in damascene features. Examples of metals that can be electroplated using provided methods include, without limitation, copper, silver, tin, indium, chromium, a tin-lead composition, a tin-silver composition, nickel, cobalt, nickel and/or cobalt alloys with each other and with tungsten, a tin-copper composition, a tin-silver-copper composition, gold, palladium, and various alloys which include these metals and compositions.
(17) In a typical electroplating process, the semiconductor wafer substrate, which may have one or more recessed features on its surface is placed into the wafer holder, and its platable (working) surface is immersed into an electrolyte contained in the electroplating bath. The wafer substrate is biased negatively, such that it serves as a cathode during electroplating. The ions of the platable metal (such as ions of metals listed above) which are contained in the electrolyte are being reduced at the surface of the negatively biased substrate during electroplating, thereby forming a layer of plated metal. The wafer, which is typically rotated during electroplating, experiences an electric field (ionic current field of the electrolyte) that may be non-uniform for a variety of reasons. This may lead to non-uniform deposition of metal. One of the types of non-uniformity is center-to-edge (or radial) non-uniformity, which manifests itself in different thicknesses of plating at different radial positions on the wafer at the same azimuthal (angular) position. Radial non-uniformity may arise from the terminal effect, due to greater amount of metal being deposited in the vicinity of electrical contacts on the wafer substrate. Because electrical contacts are made at the periphery of the wafer, around the edge of the wafer, the resistance to the flow of current in the metal seed layer, referred to as the terminal effect, manifests itself in thicker plating at the edge of the wafer substrate in comparison to the center of the substrate. One of the methods that can diminish the radial non-uniformity due to terminal effect is the use of an ionically resistive ionically permeable element positioned in close proximity of the substrate, wherein the element has an ionically permeable (e.g., porous) region that terminates at a particular radial location from the center of the element and an ionically impermeable region beyond the selected radial location. This results in inhibiting flow of ionic current through the element beyond that selected radius because the element is not permeable there. Another method, used alone or in combination, is the placement of an annular shield that blocks or diverts the plating current from the edge of the wafer substrate to a more central location.
(18) However, in many cases, dissimilar substrates, e.g., substrates that have a different distribution of recessed features on their surface will experience different distribution of plating current at their surface and may require different shields to reduce non-uniformity. Two semiconductor wafers having a different distribution of recessed features are schematically illustrated in
(19) An appropriately positioned second electrode that is configured to donate and/or divert plating current to and/or from the wafer substrate is used to modulate plating uniformity in the embodiments provided herein. The position of the electrode in relation to other components of the electroplating system is of high importance for a number of reasons including minimization of the manufacturing complexity and cost, improvement of reliability, and ease of assembly and maintainance. Two main configurations of an electroplating apparatus are shown. The configurations illustrate how the second electrode can be integrated into an electroplating system containing anolyte and catholyte compartments that are separated by a membrane. The configurations further show how a secondary electrode can be integrated with an ionically resistive ionically permeable element, such as a channeled ionically resistive plate (CIRP) positioned in the proximity of the substrate. Both configurations can be implemented in a Sabre 3D system available from Lam Research Corporation.
(20) Anolyte and Catholyte Portions of a Plating Vessel
(21) In both configurations of the apparatus provided herein the electroplating apparatus includes a plating chamber configured to hold electrolyte, where the plating chamber is separated by an ion-permeable membrane into anolyte and catholyte compartments. The primary anode is housed in the anolyte portion, while the substrate is immersed into the electrolyte in the catholyte portion across the membrane. The compositions of anolyte (electrolyte in the anolyte compartment) and catholyte (electrolyte in the catholyte compartment) can be the same or different.
(22) The membrane allows ionic communication between the anolyte and catholyte regions of the plating cell, while preventing the particles generated at the primary anode from entering the proximity of the wafer and contaminating it. In some embodiments, the membrane is a nanoporous membrane (including but not limited to reverse osmosis membrane, a cationic or anionic membrane) that is capable of substantially preventing physical movement of the solvent and of dissolved components under the influence of pressure gradients, while allowing relatively free migration of one or more charged species contained in the electrolyte via ion migration (motion in response to the application of an electric field). Detailed descriptions of suitable anodic membranes are provided in U.S. Pat. Nos. 6,126,798 and 6,569,299 issued to Reid et al., both of which are incorporated herein by reference for all purposes. Ion exchange membranes, such as cationic exchange membranes are especially suitable for these applications. These membranes are typically made of ionomeric materials, such as perfluorinated co-polymers containing sulfonic groups (e.g. Nafion), sulfonated polyimides, and other materials known to those of skill in the art to be suitable for cation exchange. Selected examples of suitable Nafion membranes include N324 and N424 membranes available from Dupont de Nemours Co. The membrane separating catholyte and anolyte may have different selectivity for different cations. For example, it may allow passage of protons at a faster rate than the passage rate of metal ions (e.g. cupric ions).
(23) Electroplating apparatus having membrane-separated catholyte and anolyte compartments achieves separation of catholyte and anolyte and allows them to have distinct compositions. For example, organic additives can be contained within catholyte, while the anolyte can remain essentially additive-free. Further, anolyte and catholyte may have differing concentrations of metal salt and acid, due, for example, to ionic selectivity of the membrane. An electroplating apparatus having a membrane is described in detail in U.S. Pat. No. 6,527,920 issued to Mayer et al., which is herein incorporated by reference for all purposes.
(24) In both configurations of the electroplating apparatus provided herein, the secondary electrode is positioned such that the plating current donated and/or diverted by the secondary electrode is not passed through the membrane separating the anolyte and catholyte portions of the plating chamber.
(25) Ionically Resistive Ionically Permeable Element
(26) In both configurations of the apparatus provided herein, the apparatus includes an ionically resistive, ionically permeable element positioned in a close proximity of the substrate in the catholyte compartment of the plating chamber. This allows for free flow and transport of electrolyte through the element, but introduces a significant ionic resistance into the plating system, and may improve center-to-edge (radial) uniformity. In some embodiments, the ionically resistive ionically permeable element further serves as a source of electrolyte flow that exits the element in a direction that is substantially perpendicular to the working face of the substrate (impinging flow), and primarily functions as a flow-shaping element. In some embodiments the element includes channels or holes that are perpendicular to the platable surface of the wafer substrate. In some embodiments the element includes channels or holes that are at an angle that is different from 90 degrees relative to the platable surface of the wafer substrate. A typical ionically resistive ionically permeable element accounts for 80% or more of the entire voltage drop of the plating cell system. In contrast, the ionically resistive ionically permeable element has very little fluid flow resistance and contributes very little to the pressure drop of the cell and ancillary supporting plumbing network system. This is due to the large superficial surface area of the element (e.g., about 12 inches in diameter or 700 cm.sup.2) and modest porosity and pore sizes (e.g. the element may have a porosity of about 1-5%) created by an appropriate number of drilled channels (also referred to as pores or holes) that may have a diameter of about 0.4 to 0.8 mm. For example, the calculated pressure drop for flowing 20 liters/minute through a porous plate having a porosity of 4.5% and thickness of 0.5 inches (e.g., a plate comprising 9600 drilled holes with 0.026 diameter) is less than 1 inch of water pressure (equal to approximately 0.036 psi). Suitable ionically resistive ionically permeable elements are described in detail, for example, in the U.S. Pat. No. 8,308,931, issued on Nov. 13, 2012, which is herein incorporated by reference in its entirety. Generally the ionically resistive ionically permeable element may include pores that form interconnecting channels within the body of the element but in many embodiments it is more preferable to use an element that has channels that do not interconnect within the body of the element (e.g., use a plate with non-interconnected drilled holes). The latter embodiment is referred to as channeled ionically resistive plate (CIRP). Two features of the CIRP are of particular importance: the placement of the CIRP in close proximity with respect to the substrate, and the fact that through-holes in the CIRP are spatially and ionically isolated from each other and do not form interconnecting channels within the body of the CIRP. Such through-holes will be referred to as 1-D through-holes because they extend in one dimension, often, but not necessarily, normal to the plated surface of the substrate (in some embodiments the 1-D holes are at an angle with respect to the wafer which is generally parallel to the CIRP front surface). These through-holes are distinct from 3-D porous networks, where the channels extend in three dimensions and form interconnecting pore structures. An example of a CIRP is a disc made of an ionically resistive material, such as polyethylene, polypropylene, polyvinylidene difluoride (PVDF), polytetrafluoroethylene, polysulphone, polyvinyl chloride (PVC), polycarbonate, and the like, having between about 6,000-12,000 1-D through-holes. The disc, in many embodiments, is substantially coextensive with the wafer (e.g., has a diameter of about 300 mm when used with a 300 mm wafer) and resides in close proximity of the wafer, e.g., just below the wafer in a wafer-facing-down electroplating apparatus. Preferably, the plated surface of the wafer resides within about 10 mm, more preferably within about 5 mm of the closest CIRP surface. In the second configuration of an apparatus that will be described herein the CIRP includes at least three segments: an inner segment configured to pass plating current from the primary anode, an outer segment configured to pass current from the secondary electrode, and a dead zone between the inner and outer segments that electrically isolates the inner and outer segments from each other and does not allow the plating currents from the primary anode and the secondary electrode to mix before they enter the CIRP or within the body of the CIRP.
(27) The presence of a resistive but ionically permeable element close to the substrate substantially reduces the impact of and compensates for the terminal effect and improves radial plating uniformity. It also simultaneously provides the ability to have a substantially spatially-uniform impinging flow of electrolyte directed upwards at the wafer surface by acting as a flow diffusing manifold plate. Importantly, if the same element is placed farther from the wafer, the uniformity of ionic current and flow improvements become significantly less pronounced or non-existent. Further, because 1-D through-holes do not allow for lateral movement of ionic current or fluid motion within the CIRP, the center-to-edge current and flow movements are blocked within the CIRP, leading to further improvement in radial plating uniformity.
(28) Another important feature of the CIRP structure is the diameter or principal dimension of the through-holes and its relation to the distance between the CIRP and the substrate. Preferably the diameter of each through-hole (or of majority of through-holes), should be no more than the distance from the plated substrate surface to the closest surface of the CIRP. Thus, the diameter or principal dimension of the through holes should not exceed 5 mm, when CIRP is placed within about 5 mm of the plated wafer surface.
(29) In some embodiments the ionically resistive ionically permeable element (e.g., a CIRP) has a top surface that is parallel to the plated surface of the substrate. In other embodiments, the top surface of the ionically resistive ionically permeable element is concave or convex.
(30) The apparatus is also configured such that the flow of the plating fluid backwards through the ionically resistive element is substantially prevented, even when the plating fluid is injected in a direction that is substantially parallel to the surface of the ionically resistive ionically permeable element. It is important to note that motion of incompressible fluids, such as water, involves various levels of scaling and balance of inertial and viscous forces. Considering the fluid dynamic Navier-Stokes equations and the fact that fluid flow behavior is governed by tensor (vector) equations with important inertial terms, one can understand that enabling the plating liquid to flow through the ionically resistive ionically permeable element from a manifold below and upwards through it may be facile (since low pressure is required to obtain a substantial amount of flow), but in contrast, fluid flowing parallel to the surface may have very little tendency and a high resistance to passing through the porous material at the same static pressure. Changing the direction of movement of fluid at a right angle from rapid movement parallel to the surface to movement that is normal to the surface involves the deceleration of the fluid and viscous dissipation of energy in the fluid, and therefore can be highly unfavorable. With that background, in other embodiments of this invention, the ionically resistive ionically permeable element has peripheral ancillary means (e.g. a fluid injector) for moving the fluid at a relatively high velocity in the direction parallel to the axis parallel to the wafer and CIRP surface, said CIRP element substantially preventing fluid from moving through the element and transiting to the exit side of elements' channels by passing into the element, through a manifold below the element and above the membrane, and then back through the element near the cross-flow exhaust side of the cell. In other words, the presence of the ionically resistive ionically permeable element combined with its pore size, porosity and parallel flow velocity, can prevent such a circumvention of the parallel flow from happening. Without wishing to be bound by any particular model or theory, it is believed that high velocity fluid has substantial amount of inertia in the direction of motion parallel to the ionically resistive element, would need to be decelerated and turn at right angle to enter the pores of the element, and as such, the ionically resistive element largely acts as a very good barrier preventing fluid from changing direction and passing through it. The two configurations of the electroplating apparatus provided herein differ in the position of the secondary electrode with respect to the ionically resistive ionically permeable element. In accordance with the first configuration provided herein, the second electrode is an azimuthally symmetrical anode (e.g., a ring) that is positioned such as to donate plating current to the substrate without passing the donated current through the ionically resistive ionically permeable element (e.g., a CIRP) and through the membrane separating the anolyte and catholyte compartments. This configuration is primarily used to control radial uniformity, but can additionally have the capability of azimuthal uniformity control, e.g., with the use of an additional azimuthally asymmetric or segmented tertiary electrode.
(31) Example of a First Configuration of an Electroplating Apparatus
(32) An illustration of a plating system of a first configuration, which employs a resistive element in close proximity to the wafer, a membrane separating anolyte and catholyte compartments, and a secondary anode is shown in
(33) Referring to
(34) The plating solution is continuously provided to plating bath 203 by a pump (not shown). In some embodiments, the plating solution flows upwards through the membrane 213 and the CIRP 219 (or other ionically resistive ionically permeable element) located in close proximity of the wafer. In other embodiments, such as when the membrane 213 is largely impermeable to flow of the plating fluid (e.g. a nanoporous media such as a cationic membrane), the plating fluid enters the plating chamber between the membrane 213 and CIRP 219, for example at the chamber periphery, and then flows through the CIRP. In this case, plating fluid within the anode chamber may be circulated and the pressure can be regulated separately from the CIRP and cathode chamber. Such separate regulation is described, for example, in the U.S. Pat. No. 8,603,305, issued Dec. 10, 2013 and in the U.S. Pat. No. 6,527,920, issued Mar. 4, 2003, both of which are herein incorporated by reference in their entireties.
(35) A secondary anode chamber 221, housing the secondary anode 223 is located on the outside of the plating vessel 203 and peripheral to the wafer. In certain embodiments, the secondary anode chamber 221 is separated from the plating bath 203 by a wall having multiple openings (a membrane support structure) covered by an ion-permeable membrane 225. The membrane allows ionic communication between the plating cell and the secondary anode chamber, thereby allowing the plating current to be donated by the second anode. The porosity of this membrane is such that it does not allow particulate material to cross from the secondary anode chamber 221 to the plating bath 203 and result in the wafer contamination. Other mechanisms for allowing fluidic and/or ionic communication between the secondary anode chamber and the main plating vessel are within the scope of this invention. Examples include designs in which the membrane, rather than an impermeable wall, provides most of the barrier between plating solution in the second cathode chamber and plating solution in the main plating vessel. A rigid framework may provide support for the membrane in such embodiments.
(36) Additionally, one or more shields, such as an annular shield 227 can be positioned within the chamber. The shields are usually ring-shaped dielectric inserts, which are used for shaping the current profile and improving the uniformity of plating, such as those described in U.S. Pat. No. 6,027,631 issued to Broadbent, which is herein incorporated by reference in its entirety and for all purposes. Of course other shield designs and shapes may be employed as are known to those of skill in the art.
(37) In general, the shields may take on any shape including that of wedges, bars, circles, ellipses and other geometric designs. The ring-shaped inserts may also have patterns at their inside diameter, which improve the ability of the shields to shape the current flux in the desired fashion. The function of the shields may differ, depending on their position in the plating cell. The apparatus of the present invention can include any of the static shields, as well as variable field shaping elements, such as those described in U.S. Pat. No. 6,402,923 issued to Mayer et al., or segmented anodes, such as described in a U.S. Pat. No. 6,497,801 issued to Woodruff et al, and U.S. Pat. No. 6,773,571 issued to Mayer et. al, each of which is herein incorporated by reference in its entirety.
(38) Two DC power supplies (not shown) can be used to control current flow to the wafer 205, the primary anode 211 and to the secondary anode 223 respectively. Alternatively, one power supply with multiple independently controllable electrical outlets can be used to provide different levels of current to the wafer and to the secondary anode. The power supply or supplies are configured to negatively bias the wafer 205 and positively bias the primary anode 211 and secondary anode 223. The apparatus further includes a controller 229, which allows modulation of current and/or potential provided to the elements of electroplating cell. The controller may include program instructions specifying current and voltage levels that need to be applied to various elements of the plating cell, as well as times at which these levels need to be changed. For example, it may include program instructions for supplying power to the secondary anode, and, optionally for dynamically varying the power supplied to the secondary anode during electroplating.
(39) Arrows show the plating current in the illustrated apparatus. Current originating from the primary anode is directed upward, passes through the membrane separating anolyte and catholyte compartments and the CIRP. Current originating from the secondary anode is directed from the periphery of the plating vessel to the center and does not pass through the membrane separating the anolyte and catholyte compartments and the CIRP.
(40) The apparatus configuration described above is an illustration of one embodiment of the present invention. Those skilled in the art will appreciate that alternative plating cell configurations that include an appropriately positioned second cathode may be used. While shielding inserts are useful for improving plating uniformity, in some embodiments they may not be required, or alternative shielding configurations may be employed. In the described configuration the plating vessel and the primary anode are substantially coextensive with the wafer substrate. In other embodiments, the diameter of the plating vessel and/or of the primary anode may be smaller than the diameter of the wafer substrate, e.g., at least about 5% smaller.
(41) Example of a Second Configuration of an Electroplating Apparatus
(42) In a second configuration of an apparatus provided herein, the secondary electrode (an anode, cathode, or an anode-cathode), which can be azimuthally symmetric or asymmetric is positioned, such that the current donated and/or diverted by such electrode does not pass through the membrane separating the anolyte and catholyte compartments, but passes through the ionically resistive ionically permeable element. A second configuration of the electroplating apparatus is illustrated in
(43) Referring again to
(44) The presence of the dead zone is associated with the need to prevent mixing of currents from the primary anode and secondary electrode. Where the inner and outer portion meet, the ionically resistive ionically permeable element must make a seal with the boundaries of the anode chamber and of the secondary electrode chamber. This is illustrated by the dead zone 231 in
(45) This arrangement can be accomplished by having a set of channels that are directed at an angle radially inward (around the inner part of the outer portion of the CIRP) and channels directed at 90 degree angle (elsewhere on the outer portion of the CIRP), wherein the outer portion of the CIRP is ionically connected to the secondary electrode flow path. In addition, in some embodiments, there may be also a set of channels on the inner portion of the CIRP that are directed at an angle radially outward (around the outer part of the inner portion of the CIRP) and channels directed at 90 degrees (elsewhere on the inner portion of the CIRP), wherein the inner portion of the CIRP is ionically connected to primary anode flow path. In some cases the channel density on the upper surface can be uniform across the entire CIRP. Because the resistance of angled channels to current flow will be greater than resistance of normally directed channels, the diameter of the angled channels may be appropriately larger than the diameter of normally directed channels to compensate for the otherwise larger resistance due to longer channel length. Alternatively the net resistance of the holes can be made the same by having only a portion of the angled hole (e.g. at the lower, or at the upper CIRP surface) having a larger diameter (with the rest of the hole being the same diameter as the standard non-angled hole). The cross-sectional view shown in
(46) Additional Features of Provided Apparatuses
(47) In some embodiments it is preferable to equip the apparatus having a first or second configuration with a manifold that provides for a cross-flow of electrolyte near the surface of the wafer. Such manifold is particularly advantageous for electroplating in relatively large recessed features, such as WLP or TSV features. In these embodiments the apparatus may include a flow shaping element positioned between the CIRP and the wafer, where the flow-shaping element provides for a cross-flow substantially parallel to the surface of the wafer substrate. For example the flow shaping element may be an omega-shaped plate that directs the cross-flow is directed towards an opening in the plate. A cross-sectional depiction of such configuration is illustrated in
(48) In some embodiments, in the second configuration, the secondary electrode chamber is positioned around the periphery of the plating vessel just above the membrane separating the catholyte and anolyte compartments of the plating vessel. In some embodiments, the part of the apparatus holding this membrane and defining the walls of the secondary electrode chamber is one integral part. An example of this part is illustrated in
(49) In some embodiments, the second electrode chamber 521 and/or the fluidic chamber 541 (either in the first or second configuration) are irrigated through one or more dedicated irrigation channels configured to deliver suitable electrolyte to the respective chambers. The composition of the electrolyte may be the same or different as the composition of catholyte in the catholyte compartment of the electroplating chamber.
(50) In some embodiments the secondary electrode chamber includes a system for removing bubbles. Such system is particularly useful, when the secondary electrode is an inert secondary anode. A portion of an apparatus containing a system for removing bubbles is illustrated in the cross sectional depiction of
(51) In some embodiments (particularly when the secondary electrode is azimuthally asymmetric), a tertiary, separately controllable, electrode for additionally controlling azimuthal uniformity may be added. The tertiary electrode may be used in conjunction with both the first and second configurations of the apparatus. The tertiary electrode in the second configuration is preferably positioned such that the current diverted and/or donated by the tertiary electrode passes through the ionically resistive ionically permeable element but does not pass through the membrane separating anolyte and catholyte compartments. The suitable tertiary electrodes include azimuthally asymmetrical and segmented anodes, cathodes and anode-cathodes, such as those described in the U.S. Pat. No. 8,858,774 by Mayer et al. titled Electroplating Apparatus for Tailored Uniformity Profile issued on Oct. 14, 2014, previously incorporated by reference.
(52) As it was mentioned above, both in the first and in the second configuration of the apparatus, the secondary electrode (e.g., an anode, a cathode, or an anode-cathode) may be separated from the substrate and catholyte compartment by an ion-permeable membrane. When an inert secondary anode is used, the membrane can prevent the transfer of bubbles from the secondary anode to the proximity of the substrate. For example, in the second configuration with an inert anode, the membrane prevents bubbles generated at the secondary inert anode from getting under the peripheral region of the CIRP, where the secondary current is confined. In other embodiments, the membrane is not used, and other methods of removing the bubbles are employed. For example, the apparatus may be configured to provide a strong flow of electrolyte in the direction opposing the bubble movement (e.g., in the direction towards the periphery of CIRP and away from the substrate). In other embodiments, instead of a membrane, the apparatus may include a directing member with a sloped surface in the proximity of the inert anode that would direct the bubbles away from the CIRP and/or the substrate. When an active (consumable) secondary anode is employed, the ionically permeable membrane between the active anode and the catholyte chamber is useful for preventing particles from being transferred from the secondary anode chamber to the catholyte chamber. In other embodiments, instead of a membrane, a high outward-directed flow of electrolyte may be used to prevent the particles from reaching the surface of the substrate. The electrolyte is returned to the plating bath after it passes through a pump and then through a filter that is configured to remove the particles.
(53) Computational Modeling
(54) The improvement in radial non-uniformity of electroplating with the use of apparatuses provided herein was validated by computational modeling, and is illustrated in
(55) A conventional apparatus includes a plating chamber separated into catholyte and anolyte compartments by an ion-selective membrane, an anode positioned in the anolyte compartment, a CIRP positioned in the catholyte compartment and an annular shield positioned below the CIRP where the annular shield had a diameter of inner opening of 274 mm. The diameter of the anode and the diameter of CIRP are substantially the same as the diameter of the wafer substrate. No secondary anode is used in the model for the conventional apparatus. The thickness of plated copper along the radius of 300 mm wafer, according to the model is shown. It can be seen from curve (a) that in a conventional apparatus the thickness of plated copper at between about 115-150 mm of the wafer radius is substantially reduced due to overshielding.
(56) An apparatus of the first configuration used in the computational model is identical to the conventional apparatus but includes a secondary anode in a secondary anode chamber that is remotely positioned around the periphery of the plating chamber and is fluidically connected with the catholyte compartment of the plating chamber such that the current donated by the second anode would not pass through the CIRP or the membrane separating the anolyte and catholyte portions of the plating chamber. The size of the primary anode, the CIRP, and the annular shield are the same as in the previous model for the conventional apparatus. During electroplating about 5-15% of the total power is applied to the secondary anode. It can be seen from curve (b) that thickness uniformity at radial positions of between about 115-140 mm is substantially improved in comparison with curve (a), and only at the near edge region (140-150 mm) the thickness of plating is increased in this model.
(57) An apparatus of the second configuration used in this configuration is identical to the conventional apparatus but includes a secondary anode in a secondary anode chamber that is remotely positioned around the periphery of the plating chamber and is fluidically connected with the catholyte compartment of the plating chamber such that the current donated by the second anode would pass through an outer portion of CIRP. The current from the secondary anode would not pass through the membrane separating the anolyte and catholyte portions of the plating chamber. In this configuration the annular shield shielding the periphery of the substrate is not used in the model, but the plating chamber housing the anode is reduced in size to about 274 mm, which is similar to the size of the primary anode. The CIRP in this model contains three portions: the inner portion configured for passing current from the primary anode has a diameter of about 274 mm, the dead zone has a width of an annulus of about 2 mm, and the outer portion configured for passing current from the secondary anode has a width of an annulus of about 8 mm. During electroplating 5-15% of the total power as applied to the secondary anode. It can be seen from curve (c) that thickness uniformity is substantially improved both in comparison with curve (a) and curve (b).
(58) Method
(59) In one aspect of the invention, an electroplating method for plating metal on dissimilar substrates, such as on semiconductor wafers having different distribution of recessed features is provided. One of such methods is illustrated in the process flow diagram shown in
(60) Dynamic control of power provided to the secondary anode can have a variety of forms. For example, power provided to the secondary anode may be gradually reduced or increased during electroplating. In other embodiments, power to the secondary anode may be turned off or turned on after a pre-determined time, e.g., corresponding to a pre-determined thickness of electroplating. Finally, both the primary and secondary anode currents can change in a fixed ratio and in concert.
(61) It is understood that the method is not limited to the use of secondary anodes and similarly can be employed with any secondary electrode as described herein. In some embodiments, the secondary electrode is azimuthally symmetric and electroplating results in a substantially azimuthally symmetric distribution of ionic current. In other embodiments, the secondary electrode is azimuthally asymmetric, or is segmented, and the method is configured to apply power to the secondary electrode (or different sections of segmented electrode) in coordination with substrate rotation, such that selected azimuthal positions on the substrate receive more or less ionic current, as desired.
(62) In other embodiments, an azimuthally asymmetric secondary electrode (in a first or second apparatus configuration) can be used to provide a substantially azimuthally symmetric current modification, and is used mainly to modify radial plating uniformity. In these methods, the substrate is typically rotated at a very high rate (e.g., of at least 100 rotations per minute), while power is applied to an azimuthally asymmetric electrode (e.g., to a C-shaped anode). At a substantially constant high rotation rate, the substrate will in general experience primarily azimuthally symmetric correction of the plating current, even when an azimuthally asymmetric secondary electrode is used.
(63) Azimuthal Uniformity
(64) As it was previously mentioned, azimuthal uniformity can be modulated using an azimuthally asymmetric or segmented secondary electrode and by energizing the electrode or its individual segments in coordination with rotation of the wafer.
(65) In some embodiments, azimuthal uniformity may be modulated by using azimuthally asymmetric shields or an azimuthally asymmetric CIRP with an ionically impermeable azimuthally asymmetric portion (e.g., a portion with no holes or blocked holes). In some implementations the rotation rate of the substrate is changed (e.g., the substrate rotates slower) when the selected azimuthal position on the wafer passes above the shield or above the ionically impermeable portion of the CIRP, thereby resulting in an increased dwell time for a selected azimuthal position in a shielded area. The use of azimuthally asymmetric shields and azimuthally asymmetric ionically resistive ionically permeable element is described in the U.S. Pat. No. 8,858,774 by Mayer et al. titled Electroplating Apparatus for Tailored Uniformity Profile issued on Oct. 14, 2014, previously incorporated by reference.
(66) The top view of one example of an azimuthally asymmetric CIRP is shown in
(67) Controller
(68) In some implementations, a controller is part of a system, which may be part of the above-described examples. Such systems can comprise semiconductor processing equipment, including a processing tool or tools, chamber or chambers, a platform or platforms for processing, and/or specific processing components (a wafer pedestal, a gas flow system, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after processing of a semiconductor wafer or substrate. The electronics may be referred to as the controller, which may control various components or subparts of the system or systems. The controller, depending on the processing requirements and/or the type of system, may be programmed to control any of the processes disclosed herein, including the parameters of delivery of power to primary anode, secondary electrode, and the substrate. Specifically, the controller may provide instructions for timing of application of power, level of power applied, etc.
(69) Broadly speaking, the controller may be defined as electronics having various integrated circuits, logic, memory, and/or software that receive instructions, issue instructions, control operation, enable cleaning operations, enable endpoint measurements, and the like. The integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and/or one or more microprocessors, or microcontrollers that execute program instructions (e.g., software). Program instructions may be instructions communicated to the controller in the form of various individual settings (or program files), defining operational parameters for carrying out a particular process on or for a semiconductor wafer or to a system. The operational parameters may, in some embodiments, be part of a recipe defined by process engineers to accomplish one or more processing steps during the fabrication of one or more layers, circuits, and/or dies of a wafer.
(70) The controller, in some implementations, may be a part of or coupled to a computer that is integrated with, coupled to the system, otherwise networked to the system, or a combination thereof. For example, the controller may be in the cloud or all or a part of a fab host computer system, which can allow for remote access of the wafer processing. The computer may enable remote access to the system to monitor current progress of fabrication operations, examine a history of past fabrication operations, examine trends or performance metrics from a plurality of fabrication operations, to change parameters of current processing, to set processing steps to follow a current processing, or to start a new process. In some examples, a remote computer (e.g. a server) can provide process recipes to a system over a network, which may include a local network or the Internet. The remote computer may include a user interface that enables entry or programming of parameters and/or settings, which are then communicated to the system from the remote computer. In some examples, the controller receives instructions in the form of data, which specify parameters for each of the processing steps to be performed during one or more operations. It should be understood that the parameters may be specific to the type of process to be performed and the type of tool that the controller is configured to interface with or control. Thus as described above, the controller may be distributed, such as by comprising one or more discrete controllers that are networked together and working towards a common purpose, such as the processes and controls described herein. An example of a distributed controller for such purposes would be one or more integrated circuits on a chamber in communication with one or more integrated circuits located remotely (such as at the platform level or as part of a remote computer) that combine to control a process on the chamber.
(71) Without limitation, example systems may include a plasma etch chamber or module, a deposition chamber or module, a spin-rinse chamber or module, a metal plating chamber or module, a clean chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an atomic layer deposition (ALD) chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, and any other semiconductor processing systems that may be associated or used in the fabrication and/or manufacturing of semiconductor wafers.
(72) As noted above, depending on the process step or steps to be performed by the tool, the controller might communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout a factory, a main computer, another controller, or tools used in material transport that bring containers of wafers to and from tool locations and/or load ports in a semiconductor manufacturing factory.
(73) Alternative Embodiments
(74) While the use of secondary electrodes was illustrated with reference to electroplating apparatuses, in some embodiments the same concepts can be applied to electroetching and electropolishing apparatuses. In these apparatuses the polarities of the anode(s) and of the cathode(s) are reversed in comparison with an electroplating apparatus. For example, the primary anode of the electroplating apparatus serves as a primary cathode of an electroetching apparatus, while the substrate is positively biased, and serves as the main anode. In these embodiments, an apparatus for electrochemically removing metal from substrates is provided, where the apparatus can be used for processing dissimilar substrates without making changes to apparatus hardware to accommodate individual substrates with differences in radial distribution of features. The apparatus may rely, in some embodiments, on a combination of mechanical and electrochemical metal removal, and includes electroetching and electropolishing apparatuses.
(75) In some embodiments an apparatus for electrochemically removing a metal on a substrate (e.g., an electroetching or electropolishing apparatus) is provided, wherein the apparatus includes: (a) a chamber configured to contain an electrolyte, the chamber comprising a catholyte compartment and an anolyte compartment (an anolyte compartment referring to the compartment housing the positively biased substrate, that serves as an anode), wherein the anolyte compartment and the catholyte compartment are separated by an ion-permeable membrane; (b) a substrate holder configured to hold the positively biased substrate in the anolyte compartment during electroplating; (c) a primary cathode positioned in the catholyte compartment of the plating chamber; (d) an ionically resistive ionically permeable element positioned between the ion-permeable membrane and the substrate holder, wherein the ionically resistive ionically permeable element is adapted to provide ionic transport through the element during electroplating; and (e) a secondary electrode configured to donate and/or divert plating current to and/or from the substrate, wherein the secondary electrode is positioned such that the donated and/or diverted plating current does not cross the ion-permeable membrane separating the anolyte and catholyte compartments, and wherein the secondary electrode is positioned such as to donate and/or divert plating current through the ionically resistive ionically permeable element.
(76) In another aspect of the invention a method of electrochemically removing metal from an anodically biased substrate is provided, wherein the method includes: (a) providing the substrate into an apparatus configured for electrochemically removing metal from the surface of the substrate, wherein the apparatus comprises: (i) a chamber configured to contain an electrolyte, the chamber comprising a catholyte compartment and an anolyte compartment, wherein the anolyte compartment and the catholyte compartment are separated by an ion-permeable membrane; (ii) a substrate holder configured to hold the substrate in the anolyte compartment during electrochemical removal of metal; (iii) a primary cathode positioned in the catholyte compartment of the plating chamber; (iv) an ionically resistive ionically permeable element positioned between the ion-permeable membrane and the substrate holder, wherein the ionically resistive ionically permeable element is adapted to provide ionic transport through the element during electrochemical metal removal; and (v) a secondary electrode configured to donate and/or divert ionic current to the substrate and/or from the substrate, wherein the secondary electrode is positioned such that the donated and/or diverted ionic current does not cross the ion-permeable membrane separating the anolyte and catholyte compartments and wherein the secondary electrode is positioned such as to donate and/or divert ionic current through the ionically resistive ionically permeable element; (b) electrochemically removing the metal from the positively biased substrate, while providing power to the secondary electrode and the primary cathode. The method may further include rotating the substrate during metal removal.
(77) In another aspect of the invention an apparatus for electrochemically removing metal from a positively biased substrate is provided, wherein the apparatus includes (a) a chamber configured to contain an electrolyte, the chamber comprising a catholyte compartment and an anolyte compartment, wherein the anolyte compartment and the catholyte compartment are separated by an ion-permeable membrane; (b) a substrate holder configured to hold the positively biased substrate in the anolyte compartment during electroplating; (c) a primary cathode positioned in the anolyte compartment of the plating chamber; (d) an ionically resistive ionically permeable element positioned between the ion-permeable membrane and the substrate holder, wherein the ionically resistive ionically permeable element is adapted to provide ionic transport through the element during electrochemical material removal; and (e) secondary electrode configured to donate and/or divert ionic current to the substrate and/or from the substrate, wherein the secondary electrode is positioned such that the donated and/or diverted ionic current does not cross the ion-permeable membrane separating the anolyte and catholyte compartments and does not cross the ionically resistive ionically permeable element. In some embodiments, in accordance with this aspect, the secondary electrode is an azimuthally symmetric secondary cathode.
(78) In another aspect of the invention a method of electrochemically removing a metal from an anodically biased substrate is provided, wherein the method includes: (a) providing the substrate into an apparatus configured for electrochemically removing metal from an anodically biased substrate, wherein the apparatus comprises: (i) a chamber configured to contain an electrolyte, the chamber comprising a catholyte compartment and an anolyte compartment, wherein the anolyte compartment and the catholyte compartment are separated by an ion-permeable membrane; (ii) a substrate holder configured to hold the substrate in the anolyte compartment during metal removal; (iii) a primary cathode positioned in the catholyte compartment of the chamber; (iv) an ionically resistive ionically permeable element positioned between the ion-permeable membrane and the substrate holder, wherein the ionically resistive ionically permeable element is adapted to provide ionic transport through the element during electrochemical removal of the metal; and (v) a secondary electrode configured to donate and/or divert ionic current to the substrate and/or from the substrate, wherein the secondary electrode is positioned such that the donated and/or diverted ionic current does not cross the ion-permeable membrane separating the anolyte and catholyte compartments and does not cross the ionically resistive ionically permeable element; (b) electrochemically removing the metal from the positively biased substrate, while providing power to the secondary electrode and the primary cathode.