The invention discloses a method for preparing leather for cases, which comprises: a. selecting cow leather, which comprises dermis layer and subcutaneous tissue layer; b. uniformly cutting the subcutaneous tissue layer as an lamellar layer, and holding it in the inner side of the cow leather; c. sculpturing the cut lamellar subcutaneous tissue layer as a desired embossed pattern, and removing its peripheral portion; d. placing the cow leather sculptured with embossed pattern in a three-dimensional mold, and pressing the embossed pattern portion towards the inner side of the dermis layer so that the raised pattern structure same with the embossed pattern is formed on the outer surface of the dermis layer; e. performing antiseptic treatment; f. performing rubber injection treatment; g. inlaying metal trim parts. With the above processing, the present invention can produce leather for cases with aesthetic style, good visual effect and noticeable feeling of touch.
Claims
1. A method for preparing leather for cases, comprising the following processing steps: selecting cow leather, which comprises a dermis layer and a subcutaneous tissue layer located in an inner side of the dermis layer; cutting out the subcutaneous tissue layer of the cow leather and uniformly cutting the cut out subcutaneous tissue layer into an lamellar subcutaneous tissue layer; embossing the lamellar subcutaneous tissue layer to form a desired embossed pattern, and removing the lamellar subcutaneous tissue layer outside a periphery of the embossed pattern; placing the dermis layer of the cow leather and the lamellar subcutaneous tissue layer embossed with the embossed pattern in a three-dimensional mold, and pressing the embossed pattern of the lamellar subcutaneous tissue layer against the inner side of the dermis layer so that portions of an outer surface of the dermis layer corresponding to the embossed pattern is raised by pressing force of the embossed pattern to form a raised pattern which is the same as the embossed pattern; and performing antiseptic treatment to the dermis layer where the raised pattern is formed.
2. A method for preparing leather for cases according to claim 1, wherein antiseptic used in the antiseptic treatment is prepared by mixing the following parts of materials by weight: sodium chloride 75 parts-80 parts; potassium sulfite 5 parts-10 parts; sodium carbonate 5 parts-10 parts; sodium fluosilicate 2 parts-3 parts; aluminum phosphide 1 parts-3 parts; 10,10-oxybisphenoxarsine 0.5 parts-2 parts.
3. A method for preparing leather for cases according to claim 2, wherein there are 80 parts of said sodium chloride, 6 parts of said potassium sulfite, 7 parts of said sodium carbonate, 3 parts of said sodium fluosilicate, 2 parts of said aluminum phosphide and 2 parts of said 10,10-oxybisphenoxarsine.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1)
DETAILED DESCRIPTION OF THE INVENTION
(2) The invention is now described with reference to the detailed embodiments.
(3) Embodiment 1, method for preparing leather for cases, comprises the processing steps as follows:
(4) a. selecting cow leather, which comprises dermis layer and subcutaneous tissue layer located in the inner side of the dermis layer;
(5) b. uniformly cutting the subcutaneous tissue layer of the cow leather as an lamellar subcutaneous tissue layer, and holding the cut lamellar subcutaneous tissue layer in the inner side of the dermis layer after the subcutaneous tissue layer of the cow leather is completely cut;
(6) c. sculpturing the cut lamellar subcutaneous tissue layer as a desired embossed pattern, and removing the subcutaneous tissue layer at outer side of the edge of the embossed pattern;
(7) d. placing the cow leather sculptured with embossed pattern in a three-dimensional mold, and pressing the embossed pattern portion at the inner side of the dermis layer so that the raised pattern structure same with the embossed pattern is formed on the outer surface of the dermis layer of the cow leather;
(8) e. performing antiseptic treatment on the cow leather formed with raised pattern structure in the dermis layer;
(9) f. performing rubber injection treatment on the subcutaneous tissue layer of the cow leather after the antiseptic treatment, wherein the injection of rubber material in the shrivelled subcutaneous tissue layer after the antiseptic treatment can effectively enhance the overall elasticity;
(10) g. inlaying metal trim parts on the outer surface of the dermis layer of the cow leather after the rubber injection treatment.
(11) With the above processing steps, the method for preparing leather for cases in the embodiment 1 can produce leather for cases with aesthetic style, good visual effect and noticeable feeling of touch.
(12) Embodiment 2, antiseptic adopted in the step e consists of the following parts of materials by weight:
(13) sodium chloride 80 parts
(14) potassium sulfite 6 parts
(15) sodium carbonate 7 parts
(16) sodium fluosilicate 3 parts
(17) aluminium phosphide 2 parts
(18) 10,10-oxybisphenoxarsine 2 parts
(19) It should be further noted that the antiseptic treatment on the cow leather can be effectively performed by the antiseptic in embodiment 2 and the antiseptic effect is good with the above material ratio. Embodiment 3, antiseptic adopted in the step e consists of the following parts of materials by weight:
(20) sodium chloride 75 parts
(21) potassium sulfite 10 parts
(22) sodium carbonate 8 parts
(23) sodium fluosilicate 3 parts
(24) aluminium phosphide 2 parts
(25) 10,10-oxybisphenoxarsine 2 parts
(26) It should be further noted that the antiseptic treatment on the cow leather can be effectively performed by the antiseptic in embodiment 3 and the antiseptic effect is good with the above material ratio.
(27) Embodiment 4, antiseptic adopted in the step e consists of the following parts of materials by weight:
(28) sodium chloride 78 parts
(29) potassium sulfite 8 parts
(30) sodium carbonate 8 parts
(31) sodium fluosilicate 2 parts
(32) aluminium phosphide 2 parts
(33) 10,10-oxybisphenoxarsine 2 parts
(34) It should be further noted that the antiseptic treatment on the cow leather can be effectively performed by the antiseptic in embodiment 4 and the antiseptic effect is good with the above material ratio.
(35) The foregoing is only preferred embodiments of the invention, various changes in particular embodiments and application areas can be made by those skilled in the art according to the principles of the invention, the disclosure should not be understood as limitation to the invention.