MULTILAYER BOARD AND MANUFACTURING METHOD THEREOF
20230309219 · 2023-09-28
Inventors
Cpc classification
B32B15/20
PERFORMING OPERATIONS; TRANSPORTING
B32B2250/42
PERFORMING OPERATIONS; TRANSPORTING
B32B2457/08
PERFORMING OPERATIONS; TRANSPORTING
B32B2270/00
PERFORMING OPERATIONS; TRANSPORTING
B32B2307/30
PERFORMING OPERATIONS; TRANSPORTING
International classification
Abstract
A multilayer board includes laminates. Each of the laminates includes a liquid crystal polymer substrate and a metal layer. Each of the liquid crystal polymer substrates has a melting point. When a number of the liquid crystal polymer substrates is an odd number, they include a first middle substrate that is located in the most middle position and has a first melting point lowest among the melting points. The melting points increase in a direction away from the first middle substrate. When the number of the liquid crystal polymer substrates is an even number, they include second and third middle substrates that are located in the most middle position and respectively have second and third melting points that are substantially same. The second or third melting point is lowest among the melting points. The melting points increase in a direction away from the second and third middle substrates.
Claims
1. A multilayer board, comprising: a plurality of laminates that are stacked from bottom to top, wherein each of the laminates is a single sided board or a double sided board and comprises a liquid crystal polymer substrate and at least one metal layer, each of the liquid crystal polymer substrates has a melting point, when a number of the liquid crystal polymer substrates is an odd number equal to or higher than 3, the liquid crystal polymer substrates comprise a first middle substrate that is located in the most middle position, a first melting point of the first middle substrate is lowest among the melting points of the liquid crystal polymer substrates, and the melting points of the liquid crystal polymer substrates increase in a direction away from the first middle substrate, when the number of the liquid crystal polymer substrates is an even number equal to or higher than 4, the liquid crystal polymer substrates comprise a second middle substrate and a third middle substrate that are located in the most middle position, a second melting point of the second middle substrate or a third melting point of the third middle substrate is lowest among the melting points of the liquid crystal polymer substrates, the second melting point and the third melting point are substantially same, and the melting points of the liquid crystal polymer substrates increase in a direction away from the second middle substrate and the third middle substrate.
2. The multilayer board of claim 1, wherein the laminates comprise: a first laminate comprising a first liquid crystal polymer substrate and at least one first metal layer, wherein the first liquid crystal polymer substrate has a fourth melting point; a second laminate comprising a second liquid crystal polymer substrate and at least one second metal layer, wherein the second liquid crystal polymer substrate has a fifth melting point; and a third laminate comprising a third liquid crystal polymer substrate and at least one third metal layer, wherein the third liquid crystal polymer substrate has a sixth melting point, wherein the second laminate is disposed between the first laminate and the third laminate, and the fourth melting point and the sixth melting point are substantially same and higher than the fifth melting point.
3. The multilayer board of claim 2, wherein the fourth melting point and the sixth melting point are 33° C. to 57° C. higher than the fifth melting point.
4. The multilayer board of claim 2, further comprising: a fourth laminate comprising a fourth liquid crystal polymer substrate and at least one fourth metal layer, wherein the fourth liquid crystal polymer substrate has a seventh melting point; and a fifth laminate comprising a fifth liquid crystal polymer substrate and at least one fifth metal layer, wherein the fifth liquid crystal polymer substrate has an eighth melting point, wherein the fourth laminate is disposed on the third laminate, the fifth laminate is disposed under the first laminate, the seventh melting point and the eighth melting point are substantially same, the seventh melting point is higher than the sixth melting point, and the eighth melting point is higher than the fourth melting point.
5. The multilayer board of claim 4, wherein the fourth melting point and the sixth melting point are 33° C. to 47° C. higher than the fifth melting point, and the seventh melting point and the eighth melting point are 43° C. to 57° C. higher than the fifth melting point.
6. The multilayer board of claim 1, wherein the laminates comprise: a first laminate comprising a first liquid crystal polymer substrate and at least one first metal layer, wherein the first liquid crystal polymer substrate has a fourth melting point; a second laminate comprising a second liquid crystal polymer substrate and at least one second metal layer, wherein the second liquid crystal polymer substrate has a fifth melting point; a third laminate comprising a third liquid crystal polymer substrate and at least one third metal layer, wherein the third liquid crystal polymer substrate has a sixth melting point; and a fourth laminate comprising a fourth liquid crystal polymer substrate and at least one fourth metal layer, wherein the fourth liquid crystal polymer substrate has a seventh melting point, wherein the first laminate, the second laminate, the third laminate, and the fourth laminate are sequentially stacked from bottom to top, the fifth melting point and the sixth melting point are substantially same, the fourth melting point and the seventh melting point are substantially same, and the fourth melting point and the seventh melting point are higher than the fifth melting point or the sixth melting point.
7. The multilayer board of claim 6, wherein the fourth melting point and the seventh melting point are 33° C. to 57° C. higher than the fifth melting point or the sixth melting point.
8. The multilayer board of claim 1, wherein the melting point of the liquid crystal polymer substrate that is closest to the first middle substrate is 33° C. to 57° C. higher than the first melting point, and the melting point of the liquid crystal polymer substrate that is closest to the second middle substrate and the third middle substrate is 33° C. to 57° C. higher than the second melting point or the third melting point.
9. The multilayer board of claim 1, wherein the liquid crystal polymer substrates comprise the same liquid crystal polymers.
10. The multilayer board of claim 1, wherein the liquid crystal polymer substrates comprise thermotropic liquid crystal polymers, thermoplastic liquid crystal polymers, or a combination thereof.
11. A method of manufacturing a multilayer board, comprising: receiving a stack, wherein the stack comprises a plurality of laminates that are stacked from bottom to top, each of the laminates is a single sided board or a double sided board and comprises a liquid crystal polymer substrate and at least one metal layer, each of the liquid crystal polymer substrates has a melting point, when a number of the liquid crystal polymer substrates is an odd number equal to or higher than 3, the liquid crystal polymer substrates comprise a first middle substrate that is located in the most middle position, a first melting point of the first middle substrate is lowest among the melting points of the liquid crystal polymer substrates, and the melting points of the liquid crystal polymer substrates increase in a direction away from the first middle substrate, when the number of the liquid crystal polymer substrates is an even number equal to or higher than 4, the liquid crystal polymer substrates comprise a second middle substrate and a third middle substrate that are located in the most middle position, a second melting point of the second middle substrate or a third melting point of the third middle substrate is lowest among the melting points of the liquid crystal polymer substrates, the second melting point and the third melting point are substantially same, and the melting points of the liquid crystal polymer substrates increase in a direction away from the second middle substrate and the third middle substrate; and pressing the stack by heat sources placed on a top surface and a bottom surface of the stack, wherein the melting point of the liquid crystal polymer substrate closest to the heat sources is T.sub.m, and a temperature of the heat sources is T.sub.m−30° C. to T.sub.m ° C.
12. The method of claim 11, wherein the laminates comprise: a first laminate comprising a first liquid crystal polymer substrate and at least one first metal layer, wherein the first liquid crystal polymer substrate has a fourth melting point; a second laminate comprising a second liquid crystal polymer substrate and at least one second metal layer, wherein the second liquid crystal polymer substrate has a fifth melting point; and a third laminate comprising a third liquid crystal polymer substrate and at least one third metal layer, wherein the third liquid crystal polymer substrate has a sixth melting point, wherein the second laminate is disposed between the first laminate and the third laminate, and the fourth melting point and the sixth melting point are substantially same and higher than the fifth melting point.
13. The method of claim 12, wherein the fourth melting point and the sixth melting point are 33° C. to 57° C. higher than the fifth melting point.
14. The method of claim 11, wherein the laminates comprise: a first laminate comprising a first liquid crystal polymer substrate and at least one first metal layer, wherein the first liquid crystal polymer substrate has a fourth melting point; a second laminate comprising a second liquid crystal polymer substrate and at least one second metal layer, wherein the second liquid crystal polymer substrate has a fifth melting point; a third laminate comprising a third liquid crystal polymer substrate and at least one third metal layer, wherein the third liquid crystal polymer substrate has a sixth melting point; and a fourth laminate comprising a fourth liquid crystal polymer substrate and at least one fourth metal layer, wherein the fourth liquid crystal polymer substrate has a seventh melting point, wherein the first laminate, the second laminate, the third laminate, and the fourth laminate are sequentially stacked from bottom to top, the fifth melting point and the sixth melting point are substantially same, the fourth melting point and the seventh melting point are substantially same, and the fourth melting point and the seventh melting point are higher than the fifth melting point or the sixth melting point.
15. The method of claim 14, wherein the fourth melting point and the seventh melting point are 33° C. to 57° C. higher than the fifth melting point or the sixth melting point.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The above mentioned or other embodiments, features, and other advantages of the present disclosure can be more clearly understood by referring to the contents of the present disclosure and the additional drawings.
[0018]
[0019]
DETAILED DESCRIPTION
[0020] The following embodiments of the present disclosure are disclosed with accompanying diagrams for detailed description. For illustration clarity, many details of practice are explained in the following descriptions. However, it should be understood that these details of practice do not intend to limit the present disclosure. That is, these details of practice are not necessary in parts of embodiments of the present disclosure. Furthermore, for simplifying the drawings, some of the conventional structures and elements are shown with schematic illustrations.
[0021] In the present disclosure, it will be understood that, although the terms first, second, third etc. may be used herein to describe various elements, components, regions, layers, and/or sections, these elements, components, regions, layers, and/or sections should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or section from another element, component, region, layer or section. Thus, a first element, component, region, layer or section discussed below could be termed a second element, component, region, layer or section without departing from the teachings of the present disclosure.
[0022] In the present disclosure, a laminate may be a single sided board or a double sided board. The single sided board includes a liquid crystal polymer substrate and a metal layer positioned on the surface of the liquid crystal polymer substrate. The double sided board includes a liquid crystal polymer substrate and two metal layers respectively positioned on the upper surface and the lower surface of the liquid crystal polymer substrate. The metal layer may be an unetched metal foil or a metal circuit formed by etching a metal foil. When the metal layer is the metal circuit, the laminate can also be referred as a circuit board.
[0023] The present disclosure provides a multilayer board that includes a plurality of laminates stacked from bottom to top. Each of the laminates is a single sided board or a double sided board. Each of the laminates includes a liquid crystal polymer substrate and at least one metal layer. Each of the liquid crystal polymer substrates has a melting point. A number of laminates is odd number or even number. When the number of the liquid crystal polymer substrates is an odd number equal to or higher than 3, the liquid crystal polymer substrates includes a first middle substrate located in the most middle position, and a first melting point of the first middle substrate is the lowest among the melting points of the liquid crystal polymer substrates, and the melting points of the liquid crystal polymer substrates increase in a direction away from the first middle substrate. In other words, the melting points of the liquid crystal polymer substrates between the first middle substrate and the upper surface of the multilayer board increases from bottom to top, and the melting points of the liquid crystal polymer substrates between the first middle substrate and the bottom surface of the multilayer board increases from top to bottom. When the number of the liquid crystal polymer substrates is an even number equal to or higher than 4, the liquid crystal polymer substrates include a second middle substrate and a third middle substrate located in the most middle positions, the second middle substrate is located on the third middle substrate. A second melting point of the second middle substrate or a third melting point of the third middle substrate is the lowest among the melting points of the liquid crystal polymer substrates. The second melting point and the third melting point are substantially same. The melting points of the liquid crystal polymer substrates increase in a direction away from the second middle substrate and the third middle substrate. In other words, the melting points of the liquid crystal polymer substrates between the second middle substrate and the upper surface of the multilayer board increases from bottom to top, and the melting points of the liquid crystal polymer substrates between the third middle substrate and the bottom surface of the multilayer board increases from top to bottom. In some embodiments, the melting points of the above middle substrates are 283° C. to 287° C., such as 283, 284, 285, 286 or 287° C. In some embodiments, the melting point of the liquid crystal polymer substrate adjacent to the above middle substrate is 33° C. to 57° C. higher than the melting point of the middle substrate, such as 33, 36, 39, 42, 45, 48, 51, 54, or 57° C.
[0024] In some embodiments, each of the liquid crystal polymer substrates includes the same kind of liquid crystal polymers. In some embodiments, each of the liquid crystal polymer substrates includes different kinds of liquid crystal polymers. In some embodiments, the liquid crystal polymer substrates include thermotropic liquid crystal polymers, thermoplastic liquid crystal polymers, or a combination thereof.
[0025] A manufacturing method of a multilayer board includes hot pressing (e.g., single hot pressing) of a stack containing the above-mentioned laminates. When fabricating the multilayer board, heat sources are placed on the top and bottom surfaces of the stack. In some embodiments, the melting point of the liquid crystal polymer substrate closest to the heat source is T.sub.m, and the temperature of the hot pressing is T.sub.m−30° C. to T.sub.m ° C. In the stack, the laminates close to the upper and lower surfaces of the stack are heated more, and the laminates farther away from the upper and lower surfaces of the stack are heated less, so the stack is unevenly heated. If the liquid crystal polymer substrates used to carry the metal layers in the laminates all include liquid crystal polymers with the same melting points, the stack may be poorly laminated due to uneven heating. However, the liquid crystal polymer substrates in the laminates of the present disclosure have different melting points, the middlemost liquid crystal polymer substrate has the lowest melting point, the outermost liquid crystal polymer substrates (i.e., the uppermost and the lowermost liquid crystal polymer substrates) have the highest melting point, and the melting points of the remaining liquid crystal polymer substrates increase outward (i.e., upward and downward). Therefore, during the hot pressing process, the deformation degrees of the liquid crystal polymer substrates are similar, so that the multilayer board formed by the stack has the advantages of good flatness and high yield. In addition, liquid crystal polymers have low water absorption, dielectric constant, loss coefficient, thermal expansion coefficient, and excellent dimensional stability, electrical properties, gas barrier properties, and thermal conductivity, so the liquid crystal polymers are more suitable as insulating substrate material for a multilayer board than ordinary dielectric materials.
[0026] Various implementation aspects of the multilayer board of the present disclosure will be described below with drawings. The number of laminates in the multilayer board of the present disclosure can be arbitrarily adjusted according to design requirements, such as 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, or 21, but not limited thereto.
[0027] As shown in
[0028] As shown in
[0029] Please refer to
TABLE-US-00001 TABLE 1 First melting point Second melting point Third melting point Example 1 M+33° C. to M + 37° C. M M + 33° C. to M + 37° C. Example 2 M+43° C. to M + 47° C. M M + 43° C. to M + 47° C. Example 3 M+53° C. to M + 57° C. M M + 53° C. to M + 57° C. Example 4 M+43° C. to M + 47° C. M + 33° C. to M + 37° C. M + 43° C. to M + 47° C. Example 5 M+53° C. to M + 57° C. M + 33° C. to M + 37° C. M + 53° C. to M + 57° C. Example 6 M+53° C. to M + 57° C. M + 43° C. to M + 47° C. M + 53° C. to M + 57° C.
[0030] In some embodiments, each of the thicknesses of the first liquid crystal polymer substrate 310A, the second liquid crystal polymer substrate 320A, and the third liquid crystal polymer substrate 330A is independently 1 um to 2000 um, such as 10 um, 50 um, 100 um, 300 um, 500 um, 700 um, 900 um, 1000 um, 1300 um, or 1500 um, but not limited thereto.
[0031] In some embodiments, conductive elements (e.g., conductive vias) (not shown) may be disposed in the first liquid crystal polymer substrate 310A, the second liquid crystal polymer substrate 320A, and the third liquid crystal polymer substrate 330A to electrically connect the metal layers. In some embodiments, the first liquid crystal polymer substrate 310A, the second liquid crystal polymer substrate 320A, and the third liquid crystal polymer substrate 330A each includes different types of liquid crystal polymers. In some embodiments, the first liquid crystal polymer substrate 310A, the second liquid crystal polymer substrate 320A, and the third liquid crystal polymer substrate 330A each includes the same type of liquid crystal polymers. In some embodiments, the first liquid crystal polymer substrate 310A, the second liquid crystal polymer substrate 320A, and the third liquid crystal polymer substrate 330A include thermotropic liquid crystal polymers, and the thermotropic liquid crystal polymers are, for example, thermotropic liquid crystal polymer resins. The thermotropic liquid crystal polymer resins include a first type high heat-resistant liquid crystal polymer resin, a second type medium heat-resistant liquid crystal polymer resin, and a third type low heat-resistant liquid crystal polymer resin.
[0032] In some embodiments, the high heat-resistant liquid crystal polymer resin includes a liquid crystal polymer resin formed by polymerizing p-hydroxybenzoic acid (HBA), terephthalic acid (TA), and 4,4′-dioxydiphenol (DODP). In other embodiments, the medium heat-resistant liquid crystal polymer resin includes a liquid crystal polymer resin formed by polymerizing p-hydroxybenzoic acid (HBA) and 6-hydroxy-2-naphthoic acid (HNA). In yet another embodiment, the low heat-resistant liquid crystal polymer resin includes a liquid crystal polymer resin formed by polymerizing polyethylene terephthalate (PET) and p-hydroxybenzoic acid (HBA).
[0033] In some embodiments, the present disclosure provides a method of adjusting a melting point of a liquid crystal polymer substrate. The liquid crystal polymer substrate includes thermotropic liquid crystal polymer resins. The melting point of the liquid crystal polymer before heating is a melting point Tm.sub.1.
[0034] In some embodiments, the melting point Tm.sub.1 is 200° C. to 400° C., such as 250, 270, 280, 290, 300, or 350° C. Step A: The liquid crystal polymer is heated to a first temperature, and the temperature is maintained at the first temperature for a first time. The first temperature is less than or equal to the first melting point of the liquid crystal polymer. In some embodiments, the difference between the first temperature and the melting point Tm.sub.1 is less than or equal to 100° C., such as 20, 40, 60, or 80° C. In some embodiments, the heating rate is 0.1° C./min to 40° C./min, such as 0.2, 0.5, 1, 5, 10, 20, 30, or 40° C./min. If the heating rate is too slow, the process time may be too long, and the manufacturing cost may be increased. If the heating rate is too fast, the liquid crystal polymer may be unevenly heated. In some embodiments, the first time is 1 minute to 48 hours, such as 1, 5, 20, or 30 minutes or 1, 5, 10, 20, 30, 40, or 48 hours. Step B: The liquid crystal polymer is cooled to a second temperature to form a modified liquid crystal polymer, in which the second temperature is lower than the first temperature. The modified liquid crystal polymer has a melting point Tm.sub.2, which is higher than the melting point Tm.sub.1 of the liquid crystal polymer. In some embodiments, the second temperature is higher than or equal to a room temperature, such as 30, 40, 50, or 60° C. In some embodiments, the second temperature is less than 100° C. Heating the liquid crystal polymer to the first temperature can partially reorganize its structure. Therefore, when the liquid crystal polymer is cooled to the second temperature, the crystal arrangement, size, and shape of the liquid crystal polymer will change, thus increasing the melting point of the liquid crystal polymer. Steps A and B can be repeatedly performed to increase the melting point of the liquid crystal polymer, and the temperature of each heating is 20° C.-50° C. higher than the temperature of the previous heating. Liquid crystal polymer substrates with different melting points can be fabricated by the above method. The liquid crystal polymer substrates may include the same or different liquid crystal polymers.
[0035] In some embodiments, the first liquid crystal polymer substrate 310A, the second liquid crystal polymer substrate 320A, and the third liquid crystal polymer substrate include thermoplastic liquid crystal polymers. In some embodiments, thermoplastic liquid crystal polymers are formed by polymerizing reactants selected from the group consisting of (1) aromatic or aliphatic dicarboxylic acids, (2) aromatic hydroxycarboxylic acids, (3) aromatic or aliphatic dihydroxy compounds, and (4) aromatic diamines, aromatic hydroxylamines, or aromatic amino carboxylic acids.
[0036] (1) The aromatic or aliphatic dicarboxylic acids include the group consisting of
##STR00001##
and HOOC(CH.sub.2).sub.nCOOH (where n is an integer from 2 to 12). (2) The aromatic hydroxycarboxylic acids include the group consisting of
##STR00002##
(X may be a hydrogen atom or a halogen atom, a low alkyl group, or a phenyl group),
##STR00003##
(3) The aromatic or aliphatic dihydroxy compounds include the group consisting of
##STR00004##
(X may be a hydrogen atom or a halogen atom, a low alkyl, or a phenyl),
##STR00005##
(Y may be O, CH.SUB.2., or S),
[0037] ##STR00006##
and HO(CH.sub.2).sub.nOH (n is an integer from 2 to 12). (4) The aromatic diamines, aromatic hydroxylamines, or aromatic amino carboxylic acids include the group consisting of
##STR00007##
[0038] The present disclosure provides a method for adjusting a melting point of a liquid crystal polymer substrate. The liquid crystal polymer substrate includes thermoplastic liquid crystal polymers. The melting point of the liquid crystal polymer substrate before heating is a melting point Tm.sub.1. A laminate is heated at a specific temperature, and the heating time is between 1 hour and 24 hours. The specific temperature is higher than or equal to Tm.sub.1−30° C. and less than Tm.sub.1, so the melting point of the liquid crystal polymer substrate in the laminate can be increased. In some embodiments, the heating time is 1, 5, 10, 15, 20, or 24 hours. By heating the laminate for a long time, the melting point of the liquid crystal polymer substrate can be raised. As the heating time increases, the melting point of the liquid crystal polymer substrate increases. Liquid crystal polymer substrates with different melting points can be fabricated by the above method. The liquid crystal polymer substrate may include the same or different liquid crystal polymers.
[0039] In some embodiments, the first metal layer 310B, the second metal layer 320B, and the third metal layer 330B are each independently a copper substrate, an aluminum substrate, a nickel substrate, a palladium substrate, or a tin substrate, but not limited thereto. For example, the metal layer may be a copper foil. In some embodiments, the thicknesses of the first metal layer 310B, the second metal layer 320B, and the third metal layer 330B are each independently 100 μm to 500 μm, such as 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, or 450 μm, but not limited thereto. In the present disclosure, all the embodiments of the liquid crystal polymer substrates and the metal layers can refer to the above embodiments of
[0040] Please refer to
[0041] Please refer to
[0042] Please refer to
[0043] As shown in
TABLE-US-00002 TABLE 2 First melting Second melting Third melting Fourth melting Fifth melting point point point point point Example 7 M + 43° C. to M + 33° C. to M M + 33° C. to M + 43° C. to M + 47° C. M + 37° C. M + 37° C. M + 47° C. Example 8 M + 43° C. to M + 33° C. to M + 33° C. to M + 53° C. to M + 47° C. M + 37° C. M + 37° C. M + 57° C. Example 9 M + 53° C. to M + 43° C. to M M + 43° C. to M + 53° C. to M + 57° C. M + 47° C. M + 47° C. M + 57° C. Example 10 M + 53° C. to M + 43° C. to M + 33° C. to M + 43° C. to M + 53° C. to M + 57° C. M + 47° C. M + 37° C. M + 47° C. M + 57° C.
[0044] As shown in
TABLE-US-00003 TABLE 3 Example 11 First melting point M + 53° C. to M + 57° C. Second melting point M + 43° C. to M + 47° C. Third melting point M + 33° C. to M + 37° C. Fourth melting point M Fifth melting point M + 33° C. to M + 37° C. Sixth melting point M + 43° C. to M + 47° C. Seventh melting point M + 53° C. to M + 57° C.
[0045] As shown in
TABLE-US-00004 TABLE 4 Example 12 First melting point M + 53° C. to M + 57° C. Second melting point M + 53° C. to M + 57° C. Third melting point M + 43° C. to M + 47° C. Fourth melting point M + 43° C. to M + 47° C. Fifth melting point M + 33° C. to M + 37° C. Sixth melting point M + 33° C. to M + 37° C. Seventh melting point M Eighth melting point M + 33° C. to M + 37° C. Ninth melting point M + 33° C. to M + 37° C. Tenth melting point M + 43° C. to M + 47° C. Eleventh melting point M + 43° C. to M + 47° C. Twelfth melting point M + 53° C. to M + 57° C. Thirteenth melting point M + 53° C. to M + 57° C.
[0046] Please refer to
[0047] Please refer to
[0048] As shown in
TABLE-US-00005 TABLE 5 Example 13 First melting point M + 53° C. to M + 57° C. Second melting point M + 43° C. to M + 47° C. Third melting point M + 33° C. o M + 37° C. Fourth melting point M Fifth melting point M + 33° C. to M + 37° C. Sixth melting point M + 43° C. to M + 47° C. Seventh melting point M + 53° C. to M + 57° C.
[0049] The present disclosure provides a multilayer board that includes multiple laminates. These laminates include multiple layers of liquid crystal polymer substrates with different melting points. The melting point of the middlemost liquid crystal polymer substrate is lowest, the melting points of the outermost liquid crystal polymer substrates are highest, and the melting points of the remaining liquid crystal polymer substrates increase outward. When hot pressing is performed on the above laminates to form a multilayer board, due to the different melting points, the deformation degrees of the liquid crystal polymer substrates are similar, so that the multilayer board has good flatness and high yield. Therefore, the multilayer board has good electrical performance.
[0050] Although the present disclosure has been described in considerable detail with reference to certain embodiments thereof, other embodiments are possible. Therefore, the spirit and scope of the appended claims should not be limited to the description of the embodiments contained herein.
[0051] It will be apparent to those skilled in the art that various modifications and variations can be made to the structure of the present disclosure without departing from the scope or spirit of the disclosure. In view of the foregoing, it is intended that the present disclosure cover modifications and variations of this disclosure provided they fall within the scope of the following claims.