Abstract
Disclosed herein are compositions, methods, and systems for supramolecular gold stripping where the composition comprises a surface-bound, linear gold anion and a solution comprising a molecular receptor that facilitates the transfer of the linear gold anion from the surface to the solution.
Claims
1. A composition comprising a surface-bound, linear gold anion and a solution, the solution comprising a molecular receptor.
2. The composition of claim 1, wherein the molecular receptor is ?-cyclodextrin (?-CD).
3. The composition of claim 1, wherein the linear gold anion is Au(CN).sub.2.sup.?.
4. The composition of claim 1, wherein the composition comprises an adduct formed from the molecular receptor and the linear gold anion.
5. The composition of claim 1, wherein the surface is the surface of activated carbon.
6. The composition of claim 1, wherein the solution is an aqueous solution
7. The composition of claim 1, wherein the solution comprising the molecular receptor at a concentration of 1-10 w/v %.
8. A method for gold stripping, the method comprising contacting a surface-bound, linear gold anion with a solution comprising a molecular receptor under conditions sufficient for transferring the linear gold anion from the surface into the solution.
9. The method of claim 8, wherein the surface-bound linear gold anion is contacted with the solution comprising the molecular receptor in the presence of a surface-bound contaminant and the linear gold-anion is selectively transferred from the surface into the solution.
10. The method of claim 8, wherein the linear gold anion is Au(CN).sub.2.sup.?.
11. The method of claim 10, wherein the contaminant is Ag(CN).sub.2.sup.?.
12. The method of claim 8, wherein the molecular receptor is ?-cyclodextrin (?-CD).
13. The method of claim 8, wherein solution comprises an adduct formed from the molecular receptor and the linear gold anion.
14. The method of claim 8, wherein the surface is the surface of activated carbon.
15. The method of claim 8, wherein the solution is an aqueous solution.
16. The method of claim 8, wherein the solution comprising the molecular receptor at a concentration of 1-10 w/v %.
17. The method of claim 8, wherein the linear gold anion is transferred from the surface into the solution at a temperature between about 10? C. and about 40? C.
18. The method of claim 8 further comprising recovering gold from the solution.
19. The method of claim 18, wherein the gold is recovered electrolytically.
20. An electrolytic system comprising an electrode and an electrolyte comprising a molecular receptor and a linear gold anion.
21. (canceled)
Description
BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Non-limiting embodiments of the present invention will be described by way of example with reference to the accompanying figures, which are schematic and are not intended to be drawn to scale. In the figures, each identical or nearly identical component illustrated is typically represented by a single numeral. For purposes of clarity, not every component is labeled in every figure, nor is every component of each embodiment of the invention shown where illustration is not necessary to allow those of ordinary skill in the art to understand the invention.
[0009]
[0010]
[0011]
[0012]
[0013]
[0014]
[0015]
[0016]
[0017]
[0018]
[0019]
[0020]
[0021]
[0022]
[0023]
[0024]
[0025]
[0026]
[0027]
[0028]
DETAILED DESCRIPTION OF THE INVENTION
[0029] Disclosed herein are gold stripping methods and compositions produced therefrom. The present technology provides for a cost-effective and energy-saving method of removing linear gold anion, such as Au(CN).sub.2.sup.?, bound to the surface of activated carbon, with an aqueous solution of environmentally benign cyclodextrin. The high binding affinity between the linear gold anion and cyclodextrin in solution enables effective molecular recognition of linear gold anion at room temperature. The gold anion containing composition obtained from performing the method can be processed subsequently to enable gold recovery by using common technologies in industry, such as electrolysis.
[0030] As demonstrated in the Examples, the binding affinity between the linear gold anion Au(CN).sub.2.sup.? and ?-cyclodextrin in aqueous solutions at room temperature can be as high as 8.1?10.sup.4 M.sup.?1. These results demonstrate that this molecular recognition process between ?-cyclodextrin and Au(CN).sub.2.sup.? can be applied to the stripping of gold from the surface of activated carbon under mild conditions using readily available ?-cyclodextrins, avoiding the traditional methods used in gold-mining protocol that employ harsh conditions and toxic chemicals. Furthermore, the Examples also demonstrate that the higher binding affinity of Au(CN).sub.2.sup.? than Ag(CN).sub.2.sup.? towards ?-cyclodextrin can be utilized to realize selective stripping for Au(CN).sub.2.sup.? in the presence of Ag(CN).sub.2.sup.?.
[0031] One aspect of the technology is a composition comprising a surface-bound, linear gold anion and a solution. The term surface-bound refers to molecules that are capable of being attached non-covalently to the surface of various materials. In some embodiments, the surface is the surface of activated carbon. The term activated carbon refers to an adsorbent derived from carbonaceous raw material, in which thermal or chemical means have been used to remove most of the volatile non-carbon constituents and a portion of the original carbon content, yielding a structure with high surface area. Activated carbon is a porous material exhibiting amphoteric characteristics and is usually used for adsorption of organic and inorganic compounds.
[0032] The term linear gold anion refers to gold-containing anions with linear geometries. The term linear refers to the molecular geometry around the central gold atom that is bonded to two other atoms is placed at a bond angle of approximately 180?. In some embodiments, the linear gold anion is Au(CN).sup.2?. The counter cations of the linear gold anions include alkaline cations such as Li.sup.+, Na.sup.+, K.sup.+, Rb.sup.+, and Cs.sup.+. In some embodiments, the counter cation is K.sup.+.
[0033] In some embodiments, the solution comprises a molecular receptor. The term molecular receptor refers to host molecules that contain a binding site or a cavity for a smaller guest molecule or an ion to bind covalently or non-covalently. In some embodiments, the molecular receptor is cyclodextrin. The term cyclodextrin refers to any of the known cyclodextrins such as unsubstituted cyclodextrins containing from six to twelve glucose units, especially, alph?-cyclodextrin, bet?-cyclodextrin, gamm?-cyclodextrin and/or their derivatives and/or mixtures thereof. The alph?-cyclodextrin consists of six glucose units, the bet?-cyclodextrin consists of seven glucose units, and the gamm?-cyclodextrin consists of eight glucose units arranged in donut-shaped rings. The specific coupling and conformation of the glucose units give the cyclodextrins rigid, conical molecular structures with hollow interiors of specific volumes. The lining of each internal cavity is formed by hydrogen atoms and glycosidic bridging oxygen atoms; therefore, this surface is fairly hydrophobic. The unique shape and physical chemical properties of the cavity enable the cyclodextrin molecules to absorb inorganic or organic molecules or parts of inorganic or organic molecules which can fit into the cavity.
[0034] In some embodiments, the molecular receptor is cyclodextrin derivatives or modified cyclodextrins. The derivatives of cyclodextrin consist mainly of molecules wherein some of the OH groups are converted to OR groups. The cyclodextrin derivatives can, for example, have one or more additional moieties that provide additional functionality, such as desirable solubility behavior and affinity characteristics. Examples of suitable cyclodextrin derivative materials include methylated cyclodextrins (e.g., RAMEB, randomly methylated bet?-cyclodextrins), hydroxyalkylated cyclodextrins (e.g., hydroxypropyl-cyclodextrin and hydroxypropyl-gamm?-cyclodextrin), acetylated cyclodextrins (e.g., acetyl-gamm?-cyclodextrin), reactive cyclodextrins (e.g., chlorotriazinyl-CD), branched cyclodextrins (e.g., glucosyl-bet?-cyclodextrin and maltosyl-cyclodextrin), sulfobutyl-cyclodextrin, and sulfated cyclodextrins.
[0035] Cyclodextrin derivatives are also disclosed in U.S. Pat. No. 6,881,712 and include, e.g., cyclodextrin derivatives with short chain alkyl groups, such as methylated cyclodextrins and ethylated cyclodextrins, wherein R is a methyl or an ethyl group; those with hydroxyalkyl substituted groups, such as hydroxypropyl cyclodextrins and/or hydroxyethyl cyclodextrins, wherein R is a CH.sub.2CH(OH)CH.sub.3 or a XH.sub.2CH.sub.2OH group; branched cyclodextrins such as maltose-bonded cyclodextrins; cationic cyclodextrins such as those containing 2-hydroxy-3-(dimethylamino)propyl ether, wherein R is CH.sub.2CH(OH)CH.sub.2N(CH.sub.3).sub.2 which is cationic at low pH; quaternary ammonium, e.g., 2-hydroxy-3-(trimethylammonio)propyl ether chloride groups, wherein R is CH.sub.2CH(OH)CH.sub.2N.sup.+(CH.sub.3).sub.3Cl.sup.?; anionic cyclodextrins such as carboxymethyl cyclodextrins, cyclodextrin sulfates, and cyclodextrin succinylates; amphoteric cyclodextrins such as carboxymethyl/quaternary ammonium cyclodextrins; cyclodextrins wherein at least one glucopyranose unit has a 3-6-anhydro-cyclomalto structure, e.g., the mono-3-6-anhydrocyclodextrins, as disclosed in Optimal Performances with Minimal Chemical Modification of Cyclodextrins, F. Diedaini-Pilard and B. Perly, The 7th International Cyclodextrin Symposium Abstracts, April 1994, p. 49 said references being incorporated herein by reference; and mixtures thereof. Other cyclodextrin derivatives are disclosed in U.S. Pat. No. 3,426,011, Parmerter et al., issued Feb. 4, 1969; U.S. Pat. Nos. 3,453,257; 3,453,258; 3,453,259; and 3,453,260, all in the names of Parmerter et al., and all issued Jul. 1, 1969; U.S. Pat. No. 3,459,731, Gramera et al., issued Aug. 5, 1969; U.S. Pat. No. 3,553,191, Parmerter et al., issued Jan. 5, 1971; U.S. Pat. No. 3,565,887, Parmerter et al., issued Feb. 23, 1971; U.S. Pat. No. 4,535,152, Szejtli et al., issued Aug. 13, 1985; U.S. Pat. No. 4,616,008, Hirai et al., issued Oct. 7, 1986; U.S. Pat. No. 4,678,598, Ogino et al., issued Jul. 7, 1987; U.S. Pat. No. 4,638,058, Brandt et al., issued Jan. 20, 1987; and U.S. Pat. No. 4,746,734, Tsuchiyama et al., issued May 24, 1988; all of said patents being incorporated herein by reference.
[0036] In some embodiments, the molecular receptor is ?-cyclodextrin. As used herein, the term ?-cyclodextrin refers to a cyclic oligosaccharide consisting of six glucose subunits joined by ?-(1,4) glycosidic bonds forming the shape of a tapered cylinder as shown in
##STR00001##
[0037] In some embodiments, the composition comprises an adduct formed from the molecular receptor and the linear gold anion. As used herein, an adduct is a new chemical species AB, each molecular entity of which is formed by direct combination of two separate molecular entities A and B in such a way that there is change in connectivity, but no loss, of atoms within the moieties A and B. Stoichiometries other than 1:1 are also possible, such as 2:1, 3:1, 4:1 and so forth. In some embodiments, the adduct is formed from a linear gold anion non-covalently bound to the cavity of ?-cyclodextrin.
[0038] The solution is selected to allow for the transfer of the linear gold anion from the surface into solution. In some embodiments, the solution is an aqueous solution.
[0039] The concentration of molecular receptor may be selected by those of skill in the art based on several different factors, such as the amount of surface-bound gold to be transferred into solution. Other factors may include, without limitation, the solvent present, the counterions present, the presence and/or amount of contaminants present, the temperature at which transferring step is performed, whether the transferring step is performed in a single or multiple stages, whether the transferring step is performed in a batch or continuous process, and the like. Generally, higher concentrations of the molecular receptor allow for more gold to be transferred into solution. In some embodiments, the solution comprises the molecular receptor at a concentration of 1-10 w/v %. In some embodiments, the solution comprises the molecular receptor at a concentration of at least greater than 1 w/v %, at least 1.5 w/v %, at least 2 w/v %, at least 2.5 w/v %, at least 3 w/v %, at least 3.5 w/v %, at least 4 w/v %, at least 4.5 w/v %, at least 5 w/v %, at least 5.5 w/v %, at least 6 w/v %, at least 6.5 w/v %, at least 7 w/v %, at least 7.5 w/v %, at least 8 w/v %, at least 8.5 w/v %, at least 9 w/v %, or at least 9.5 w/v %.
[0040] Another aspect of the technology is to provide a method for gold stripping. The method comprises contacting a surface-bound, linear gold anion as described herein with a solution comprising a molecular receptor as described herein under conditions sufficient for transferring the linear gold anion from the surface into the solution. The conditions may generally refer to the chemical environment or processing conditions.
[0041] Chemical environment may refer to the amount of surface-bound gold, the concentration of the molecular receptor, the amount and/or type of surface onto which the gold is bound, the solvent, the presence or amount of contaminants, and the like.
[0042] Processing conditions may refer to the temperature at which the temperature at which the transferring step is performed, the pressure at which the transferring is being performed, the volumes being processed, whether the transferring step is performed in a single or multiple stages, whether the transferring step is performed in a batch or continuous process, and the like.
[0043] An advantage of the present technology is that the transferring step may be performed without the need for harsh conditions, high temperatures, high pressures, or concentrated cyanide or hydroxide solutions.
[0044] The transferring step may be performed at moderate temperatures. Moderate temperatures refers to temperatures between 0? C. and 50? C. In some embodiments, the transferring occurs at a temperature between about 10? C. and about 40? C. In some embodiments, the linear gold anion is transferred from the surface into the solution at a temperature between about 15? C. and about 35? C., between about 20? C. and about 30? C., or between about 23? C. and about 27? C.
[0045] Another aspect of the technology is to provide a method for selective gold stripping from a surface. The method comprises contacting a composition comprising a surface-bound, linear gold anion and an anionic contaminant with a solution comprising a molecular receptor under conditions sufficient for selectively transferring the linear gold anion from the surface into the solution. Selectively transferring the linear gold anion refers to a selectivity for the linear gold anion over the contaminant of 10:1 or more. In some embodiments, the selectivity for the linear gold anion is greater than 15:1, 20:1, 25:1, or 30:1. Thus the methods disclosed herein allow for the recovery of gold where contaminants may be present in the source of gold or that result in the course of the processing or recovery of gold.
[0046] The contaminant may be a linear metal anion. In some embodiments, the contaminant and the linear gold anion differ by the substitution of the gold atom with another metal. Accordingly, the linear gold anion and contaminant may comprise the same ligands surrounding a central metal atom with substantially the same orientation. In some embodiments, the linear gold anion is Au(CN).sub.2.sup.? and the contaminant is Ag(CN).sub.2.sup.?.
[0047] In some embodiments, the contaminant is bound to the surface of activated carbon. In some embodiments, the contaminant is bound to the same surface on which the linear gold anion is bound. In some embodiments, the contaminant is bound to a different surface than which the linear gold anion is bound.
[0048] In some embodiments, the method further comprises recovering gold from the solution. In some embodiments, the gold is recovered electrolytically. Electrolytic processes of recovering gold from solution have been described, e.g., in Nehl et al. Selective electrowinning of silver and gold from cyanide process solutions. United States: N. p., 1993.
[0049] Electrowinning, also called electroextraction, is the electrodeposition of metals that have been put in solution. Electrowinning uses electroplating purification of metals. In electrowinning, an electrical current is passed from an inert anode (oxidation) through a solution containing the dissolved metal ions so that the metal is recovered as it is deposited in an electroplating process onto the cathode (reduction). The metal ions migrate through the electrolyte towards the cathode where the pure metal is deposited.
[0050] Another aspect of the technology is to provide an electrolytic system. The electrolytic system comprises an electrode and an electrolyte comprising a molecular receptor and a linear gold anion. The electrode and potential applied to the electrode should be selected to allow for the deposition of the gold from solution. In some embodiment, the electrolyte comprises the compositions as described herein.
[0051] The above aspects of the technology are illustrated in detail in the following exemplary embodiments of the invention, which finds applications in gold stripping processes that can be conducted at room temperature and in the absence of harsh or toxic chemicals. In order to achieve room temperature stripping of gold, a molecular receptor is utilized for Au(CN).sub.2.sup.? in aqueous solution to facilitate (
[0052] Single crystals of a 1:1 adduct were obtained by slow evaporation of an aqueous solution containing a mixture of ?-CD and KAu(CN).sub.2. We note that ?-CD (100 mM) requires heat for it to dissolve in H.sub.2O. In the presence of KAu(CN).sub.2, ?-CD dissolves instantly, suggesting that complexation is occuring. The solid-state superstructure of the 1:1 adduct between ?-CD and Au(CN).sub.2.sup.? is illustrated in
TABLE-US-00001 TABLE 1 The Intermolecular Distances.sup.a Between KAu(CN).sub.2 and ?-CD in The Solid-State Superstructures With 1:1 and 1:2 Stoichiometries. Distances/? [AuH-5] [AuH-6] [NCH-3] [CNH-3] [CNH-5] [K.sup.+O] Au(CN).sub.2.sub.
[0053] Single crystals of a 2:1 adduct were also obtained (
[0054] The association between ?-CD and KAu(CN).sub.2 in D.sub.2O was investigated by .sup.1H NMR titrations. Inner protons H-3 and H-5 (
[0055] In order to shed more light on the driving force for the 1:1 adduct formation between Au(CN).sub.2.sup.? and ?-CD in water, isothermal titration calorimetry (ITC) was performed at 25? C. A stock aqueous solution of ?-CD in a syringe was titrated into an aqueous solution of KAu(CN).sub.2 (0.5 mM) placed in a titration cell. The molecular recognition between ?-CD and Au(CN).sub.2.sup.? is accompanied (
[0056] The binding affinity (K.sub.a=1.4?10.sup.3 M.sup.?1) between Ag(CN).sub.2.sup.? (
[0057] The decrease in binding affinity of ?-CD for Ag(CN).sub.2.sup.? in H.sub.2O is the result of a larger entropic penalty associated with a T?S value of ?3.7 kcal mol.sup.?1, which can be attributable to the difference in hydration states of the Au(CN).sub.2.sup.? and Ag(CN).sub.2.sup.? ions in water. This result suggests that the binding of Au(CN).sub.2.sup.? in water is most likely aided and abetted by hydrophobic effects.sup.97-99 that provide a favorable binding enthalpy by (i) releasing high-energy water from inside the ?-CDs (ii) while reducing the entropic penalty resulting from the transfer of surface-bound water from the CDs and Au(CN).sub.2.sup.? anions into the bulk solution.
[0058] The high affinity of ?-CD for Au(CN).sub.2.sup.? anions in H.sub.2O can be applied as a stripping agent to remove Au from the surface of activated carbon at room temperature. The Au-stripping experiments were performed at room temperature. An aqueous solution (5 mL) of ?-CD at a range of concentrations (1-10% w/v) was mixed with Au-loaded carbon (50 mg, containing 0.6 mg Au) and the suspension was stirred for 30 min, after which time the carbon was isolated by filtration. The concentration of Au in the filtrate was determined by inductively coupled plasma mass spectrometry. The concentration of the stripped Au increases (
[0059] Ag stripping using the same protocol was also tested. Compared with Au, the recovery (
[0060] The Examples demonstrate that molecular recognition of Au(CN).sub.2.sup.? by ?-cyclodextrin in aqueous solution with a binding affinity in the order of 10.sup.4 M.sup.?1. The binding is driven by a favorable enthalpy against a small entropic penalty. The 1:1 and 2:1 adducts, respectively, between ?-cyclodextrin and KAu(CN).sub.2 are sustained by multiple [CH . . . ?] and [CH . . . Anion] interactions in addition to hydrophobic effects. The Examples also demonstrate that the molecular recognition between ?-cyclodextrin and Au(CN).sub.2.sup.? can be applied to strip gold from the surface of activated carbon at room temperature. We also show that ?-cyclodextrin can strip selectively Au(CN).sub.2.sup.? in the presence of Ag(CN).sub.2.sup.?, a process that is difficult to achieve using the current carbon-in-pulp process. These findings allow for integration into commercial gold-mining protocols and lead to significantly reduced costs, energy consumption, and environmental impact.
[0061] Unless otherwise specified or indicated by context, the terms a, an, and the mean one or more. For example, a molecule should be interpreted to mean one or more molecules.
[0062] As used herein, about, approximately, substantially, and significantly will be understood by persons of ordinary skill in the art and will vary to some extent on the context in which they are used. If there are uses of the term which are not clear to persons of ordinary skill in the art given the context in which it is used, about and approximately will mean plus or minus ?10% of the particular term and substantially and significantly will mean plus or minus >10% of the particular term.
[0063] As used herein, the terms include and including have the same meaning as the terms comprise and comprising. The terms comprise and comprising should be interpreted as being open transitional terms that permit the inclusion of additional components further to those components recited in the claims. The terms consist and consisting of should be interpreted as being closed transitional terms that do not permit the inclusion additional components other than the components recited in the claims. The term consisting essentially of should be interpreted to be partially closed and allowing the inclusion only of additional components that do not fundamentally alter the nature of the claimed subject matter.
[0064] All methods described herein can be performed in any suitable order unless otherwise indicated herein or otherwise clearly contradicted by context. The use of any and all examples, or exemplary language (e.g., such as) provided herein, is intended merely to better illuminate the invention and does not pose a limitation on the scope of the invention unless otherwise claimed. No language in the specification should be construed as indicating any non-claimed element as essential to the practice of the invention.
[0065] All references, including publications, patent applications, and patents, cited herein are hereby incorporated by reference to the same extent as if each reference were individually and specifically indicated to be incorporated by reference and were set forth in its entirety herein.
[0066] Preferred aspects of this invention are described herein, including the best mode known to the inventors for carrying out the invention. Variations of those preferred aspects may become apparent to those of ordinary skill in the art upon reading the foregoing description. The inventors expect a person having ordinary skill in the art to employ such variations as appropriate, and the inventors intend for the invention to be practiced otherwise than as specifically described herein. Accordingly, this invention includes all modifications and equivalents of the subject matter recited in the claims appended hereto as permitted by applicable law. Moreover, any combination of the above-described elements in all possible variations thereof is encompassed by the invention unless otherwise indicated herein or otherwise clearly contradicted by context.
REFERENCES
[0067] (1) Gold Ore Processing: Project Development and Operations; Adams, M. D., Ed.; Elsevier: Singapore, 2016. [0068] (2) Hutchings, G. J.; Brust, M.; Schmidbaur, H. Gold-An Introductory Perspective. Chem. Soc. Rev. 2008, 37, 1759-1765. [0069] (3) Gorin, D. J.; Toste, F. D. Relativistic Effects in Homogeneous Gold Catalysis. Nature 2007, 446, 395-403. [0070] (4) Puddephatt, R. J. Macrocycles, Catenanes, Oligomers and Polymers in Gold Chemistry. Chem. Soc. Rev. 2008, 37, 2012-2027. [0071] (5) Corma, A.; Garci, H. Supported Gold Nanoparticles as Catalysts for Organic Reactions. Chem. Soc. Rev. 2008, 37, 2096-2126. [0072] (6) Goldup, S. M.; Leigh, D. A.; Lusby, P. J.; McBurney, R. T.; Slawin, A. M. Z. Gold (I)-Template Catenane and Rotaxane Synthesis. Angew. Chem. Int. Ed. 2008, 47, 6999-7003. [0073] (7) Galli, M.; Lewis, J. E. M.; Goldup, S. M. A Stimuli-Responsive Rotaxane-Gold Catalyst: Regulation of Activity and Diastereoselectivity. Angew. Chem. Int. Ed. 2015, 54, 13545-13549. [0074] (8) Pfl?sterer, D.; Hashmi, A. S. K. Gold Catalysis in Total Synthesis-Recent Achievements. Chem. Soc. Rev. 2016, 45, 1331-1367. [0075] (9) Lewis, J. E. M.; Beer, P. D.; Loeb, S. J.; Goldup, S. M. Metal Ions in the Synthesis of Interlocked Molecules and Materials. Chem. Soc. Rev. 2017, 46, 2577-2591. [0076] (10) Taschinski, S.; D?pp, R.; Ackermann, M.; Rominger, F.; de Vries, F.; Menger, M. F. S. J.; Rudolph, M.; Hashmi, A. S. K.; Klein, J. E. M. N. Light-Induced Mechanistic Divergence in Gold(I) Catalysis: Revisiting the Reactivity of Diazonium Salts. Angew. Chem. Int. Ed. 2019, 58, 16988-16993. [0077] (11) Grzelczak, M.; P?rez-Juste, J.; Mulvaney, P.; Liz-Marz?n, L. M. Shape Control in Gold Nanoparticle Synthesis. Chem. Soc. Rev. 2008, 37, 1783-1791. [0078] (12) Giljohann, D. A.; Seferos, D. S.; Daniel, W. L.; Massich, M. D.; Patel, P. C.; Mirkin, C. A. Gold Nanoparticles for Biology and Medicine. Angew. Chem. Int. Ed. 2010, 49, 3280-3294. [0079] (13) Saha, K.; Agasti, S. S.; Kim, C.; Li, X.; Rotello, V. M. Gold Nanoparticles in Chemical and Biological Sensing. Chem. Rev. 2012, 112, 2739-2779. [0080] (14) Personick, M. L.; Mirkin, C. A. Making Sense of the Mayhem Behind Shape Control in the Synthesis of Gold Nanoparticles. J. Am. Chem. Soc. 2013, 135, 18238-18247. [0081] (15) Bishop, P. T.; Ashfield, L. J.; Berzins, A.; Boardman, A.; Buche, V.; Cookson, J.; Gordon, R. J.; Salcianu, C.; Sutton, P. A. Printed Gold for Electronic Applications. Gold Bull. 2010, 43, 181-188. [0082] (16) Goodman, P. Current and Future Uses of Gold in Electronics. Gold Bull. 2002, 35, 21-26. [0083] (17) Online, V. Biological Applications of Gold Nanoparticles. Chem. Soc. Rev. 2008, 37, 1909-1930. [0084] (18) Boisselier, E.; Astruc, D. Gold Nanoparticles in Nanomedicine: Preparations, Imaging, Diagnostics, Therapies and Toxicity. Chem. Soc. Rev. 2009, 38, 1759-1782. [0085] (19) Yang, Z.; Jiang, G.; Xu, Z.; Zhao, S.; Liu, W. Advances in Alkynyl Gold Complexes for Use as Potential Anticancer Agents. Coord. Chem. Rev. 2020, 423, 213492. [0086] (20) Hilson, G.; Monhemius, A. J. Alternatives to Cyanide in the Gold Mining Industry: What Prospects for the Future? J. Clean. Prod. 2006, 14, 1158-1167. [0087] (21) Hagel?ken, C.; Corti, C. W. Recycling of Gold from Electronics: Cost-Effective Use through Design for Recycling. Gold Bull. 2010, 43, 209-220. [0088] (22) Syed, S. Recovery of Gold from Secondary SourcesA Review. Hydrometallurgy 2012, 115-116, 30-51. [0089] (23) Nelson, J. J. M.; Schelter, E. J. Sustainable Inorganic Chemistry: Metal Separations for Recycling. Inorg. Chem. 2019, 58, 979-990. [0090] (24) Rao, M. D.; Singh, K. K.; Morrison, C. A.; Love, J. B. Challenges and Opportunities in the Recovery of Gold from Electronic Waste. RSC Adv. 2020, 10, 4300-4309. [0091] (25) Adams, M. D. The Mechanism of Adsorption of Aurocyanide onto Activated Carbon, 1. Relation between the Effects of Oxygen and Ionic Strength. Hydrometallurgy 1990, 25, 171-184. [0092] (26) Adams, M. D.; McDougall, G. J.; Hancock, R. D. Models for the Adsorption of Aurocyanide onto Activated Carbon. Part II: Extraction of Aurocyanide Ion Pairs by Polymeric Adsorbents. Hydrometallurgy 1987, 18, 139-154. [0093] (27) Zadra, J. B. A Process for the Recovery of Gold from Activated Carbon by Leaching and Electrolysis; Report of Investigations/United States Department of the Interior, Bureau of Mines; U.S. Department of the Interior, Bureau of Mines, 1950. [0094] (28) Ubaldini, S.; Massidda, R.; Vegli?, F.; Beolchini, F. Gold Stripping by Hydro-Alcoholic Solutions from Activated Carbon: Experimental Results and Data Analysis by a Semi-Empirical Model. Hydrometallurgy 2006, 81, 40-44. [0095] (29) Soleimani, M.; Kaghazchi, T. Gold Recovery from Loaded Activated Carbon Using Different Solvents. J. Chinese Inst. Chem. Eng. 2008, 39, 9-11. [0096] (30) Bunney, K.; Jeffrey, M. I.; Pleysier, R.; Breuer, P. L. Selective Elution of Gold, Silver and Mercury Cyanide from Activated Carbon. Miner. Metall. Process. 2010, 27, 205-211. [0097] (31) Liu, Z.; Frasconi, M.; Lei, J.; Brown, Z. J.; Zhu, Z.; Cao, D.; Iehl, J.; Liu, G.; Fahrenbach, A. C.; Botros, Y. Y.; Farha, O. K.; Hupp, J. T.; Mirkin, C. A.; Stoddart, J. F. Selective Isolation of Gold Facilitated by Second-Sphere Coordination with a-Cyclodextrin. Nat. Commun. 2013, 4, 1855. [0098] (32) Liu, Z.; Samanta, A.; Lei, J.; Sun, J.; Wang, Y.; Stoddart, J. F. Cation-Dependent Gold Recovery with ?-Cyclodextrin Facilitated by Second-Sphere Coordination. J. Am. Chem. Soc. 2016, 138, 11643-11653. [0099] (33) Fissaha, H. T.; Torrejos, R. E. C.; Kim, H.; Chung, W. J.; Nisola, G. M. Thia-Crown Ether Functionalized Mesoporous Silica (SBA-15) Adsorbent for Selective Recovery of Gold (Au.sup.3+) Ions from Electronic Waste Leachate. Microporous Mesoporous Mater. 2020, 305, 110301. [0100] (34) Lin, R.-L.; Dong, Y.-P.; Tang, M.; Liu, Z.; Tao, Z.; Liu, J.-X. Selective Recovery and Detection of Gold with Cucurbit[n]urils (n=5-7). Inorg. Chem. 2020, 59, 3850-3855. [0101] (35) Chen, L.-X.; Liu, M.; Zhang, Y.-Q.; Zhu, Q.-J.; Liu, J.-X.; Zhu, B.-X.; Tao, Z. Outer Surface Interactions to Drive Cucurbit[8]uril-Based Supramolecular Frameworks: Possible Application in Gold Recovery. Chem. Commun. 2019, 55, 14271-14274. [0102] (36) Wu, H.; Jones, L. O.; Wang, Y.; Shen, D.; Liu, Z.; Zhang, L.; Cai, K.; Jiao, Y.; Stern, C. L.; Schatz, G. C.; Stoddart, J. F. High-Efficiency Gold Recovery Using Cucurbit[6]uril. ACS Appl. Mater. Interfaces 2020, 12, 38768-38777. [0103] (37) Serpell, C. J.; Cookson, J.; Ozkaya, D.; Beer, P. D. Core@shell Bimetallic Nanoparticle Synthesis via Anion Coordination. Nat. Chem. 2011, 3, 478-483. [0104] (38) Wang, L.-L.; Tu, Y.-K.; Yao, H.; Jiang, W. 2,3-Dibutoxynaphthalene-Based Tetralactam Macrocycles for Recognizing Precious Metal Chloride Complexes. Beilstein J. Org. Chem. 2019, 15, 1460-1467. [0105] (39) Doidge, E. D.; Carson, I.; Tasker, P. A.; Ellis, R. J.; Morrison, C. A.; Love, J. B. A Simple Primary Amide for the Selective Recovery of Gold from Secondary Resources. Angew. Chem. Int. Ed. 2016, 55, 12436-12439. [0106] (40) Liu, W.; Oliver, A. G.; Smith, B. D. Macrocyclic Receptor for Precious Gold, Platinum, or Palladium Coordination Complexes. J. Am. Chem. Soc. 2018, 140, 6810-6813. [0107] (41) Doidge, E. D.; Kinsman, L. M. M.; Ji, Y.; Carson, I.; Duffy, A. J.; Kordas, I. A.; Shao, E.; Tasker, P. A.; Ngwenya, B. T.; Morrison, C. A.; Love, J. B. Evaluation of Simple Amides in the Selective Recovery of Gold from Secondary Sources by Solvent Extraction. ACS Sustain. Chem. Eng. 2019, 7, 15019-15029. [0108] (42) Shaffer, C. C.; Liu, W.; Oliver, A. G.; Smith, B. D. Supramolecular Paradigm for Capture and Co-Precipitation of Gold(III) Coordination Complexes. Chem. Eur. J. 2020, doi: 10.1002/chem.202003680. [0109] (43) Dai, Y.; Zheng, K.; Tan, Y.; Xiang, W.; Xianyu, B.; Xu, H. Fischesserite-Inspired Recyclable Se-Polyurethanes for Selective Gold Extraction. Adv. Sustain. Syst. 2020, 4, 1-6. [0110] (44) Dong, C.-C.; Xiang, J.-F.; Xu, L.-J.; Gong, H.-Y. MCl4.sup.n? (AuCl.sub.4.sup.?, PtCl.sub.4.sup.2?, or PdCl.sub.4.sup.2?) Anion Extraction from Na.sub.nMCl.sub.4 in Water Using a Tetraimidazolium Macrocyclic Receptor. Tetrahedron Lett. 2018, 59, 264-267. [0111] (45) Sun, D. T.; Gasilova, N.; Yang, S.; Oveisi, E.; Queen, W. L. Rapid, Selective Extraction of Trace Amounts of Gold from Complex Water Mixtures with a Metal-Organic Framework (MOF)/Polymer Composite. J. Am. Chem. Soc. 2018, 140, 16697-16703. [0112] (46) Zhou, S.; Hu, C.; Xu, W.; Mo, X.; Zhang, P.; Liu, Y.; Tang, K. Fast Recovery of Au(III) and Ag(I) via Amine-Modified Zeolitic Imidazolate Framework-8. Appl. Organomet. Chem. 2020, 34, e5541. [0113] (47) Wang, C.; Lin, G.; Zhao, J.; Wang, S.; Zhang, L. Enhancing Au(III) Adsorption Capacity and Selectivity via Engineering MOF with Mercapto-1,3,4-thiadiazole. Chem. Eng. J. 2020, 388, 124221. [0114] (48) Nguyen, T. S.; Hong, Y.; Dogan, N. A.; Yavuz, C. T. Gold Recovery from e-Waste by Porous Porphyrin-Phenazine Network Polymers. Chem. Mater. 2020, 32, 5343-5349. [0115] (49) Ma, T.; Zhao, R.; Li, Z.; Jing, X.; Faheem, M.; Song, J.; Tian, Y.; Lv, X.; Shu, Q.; Zhu, G. Efficient Gold Recovery from e-Waste via a Chelate-Containing Porous Aromatic Framework. ACS Appl. Mater. Interfaces 2020, 12, 30474-30482. [0116] (50) Hong, Y.; Thirion, D.; Subramanian, S.; Yoo, M.; Choi, H.; Kim, H. Y.; Stoddart, J. F.; Yavuz, C. T. Precious Metal Recovery from Electronic Waste by a Porous Porphyrin Polymer. Proc. Natl. Acad. Sci. USA 2020, 117, 16174-16180. [0117] (51) Snowden, T. S.; Anslyn, E. V. Anion Recognition: Synthetic Receptors for Anions and Their Application in Sensors. Curr. Opin. Chem. Biol. 1999, 3, 740-746. [0118] (52) Kubik, S. Anion Recognition in Water. Chem. Soc. Rev. 2010, 39, 3648-3663. [0119] (53) Xu, Z.; Kim, S. K.; Yoon, J. Revisit to Imidazolium Receptors for the Recognition of Anions: Highlighted Research during 2006-2009. Chem. Soc. Rev. 2010, 39, 1457-1466. [0120] (54) Brotherhood, P. R.; Davis, A. P. Steroid-Based Anion Receptors and Transporters. Chem. Soc. Rev. 2010, 39, 3633-3647. [0121] (55) Busschaert, N.; Caltagirone, C.; Van Rossom, W.; Gale, P. A. Applications of Supramolecular Anion Recognition. Chem. Rev. 2015, 115, 8038-8155. [0122] (56) Flood, A. H. Creating Molecular Macrocycles for Anion Recognition. Beilstein J. Org. Chem. 2016, 12, 611-627. [0123] (57) Liu, Y.; Sengupta, A.; Raghavachari, K.; Flood, A. H. Anion Binding in Solution: Beyond the Electrostatic Regime. Chem 2017, 3, 411-427. [0124] (58) Kubik, S. Anion Recognition in Aqueous Media by Cyclopeptides and Other Synthetic Receptors. Acc. Chem. Res. 2017, 50, 2870-2878. [0125] (59) He, Q.; Tu, P.; Sessler, J. L. Supramolecular Chemistry of Anionic Dimers, Trimers, Tetramers, and Clusters. Chem 2018, 4, 46-93. [0126] (60) He, Q.; Vargas-Z??iga, G. I.; Kim, S. H.; Kim, S. K.; Sessler, J. L. Macrocycles as Ion Pair Receptors. Chem. Rev. 2019, 119, 9753-9835. [0127] (61) Chen, L.; Berry, S. N.; Wu, X.; Howe, E. N. W.; Gale, P. A. Advances in Anion Receptor Chemistry. Chem 2020, 6, 61-141. [0128] (62) Hein, R.; Beer, P. D.; Davis, J. J. Electrochemical Anion Sensing: Supramolecular Approaches. Chem. Rev. 2020, 120, 1888-1935. [0129] (63) Wang, D.-X.; Wang, M.-X. Exploring Anion-x Interactions and Their Applications in Supramolecular Chemistry. Acc. Chem. Res. 2020, 53, 1364-1380. [0130] (64) Pancholi, J.; Beer, P. D. Halogen Bonding Motifs for Anion Recognition. Coord. Chem. Rev. 2020, 416, 213281. [0131] (65) Wu, X.; Gilchrist, A. M.; Gale, P. A. Prospects and Challenges in Anion Recognition and Transport. Chem 2020, 6, 1296-1309. [0132] (66) Canumalla, A. J.; Schraa, S.; Isab, A. A.; Shaw, C. F.; Gleichmann, E.; Dunemann, L.; Turfeld, M. Equilibrium Binding Constants and Facile Dissociation of Novel Serum Albumin-Dicyanoaurate(I) Complexes. J. Biol. Inorg. Chem. 1998, 3, 9-17. [0133] (67) Pham, D. M.; Rios, D.; Olmstead, M. M.; Balch, A. L. Assisted Self-Association of Dicyanoaurate, [Au(CN).sub.2].sup.?, and Dicyanoargentate, [Ag(CN).sub.2].sup.?, Through Hydrogen Bonding to Metal Ammonia Complexes. Inorg. Chim. Acta 2005, 358, 4261-4269. [0134] (68) Moriuchi, T.; Yoshii, K.; Katano, C.; Hirao, T. Luminescent Properties of Dicyanoaurate(I) Aggregates Based on Electrostatic Assembly along Poly(Allylamine Hydrochloride). Tetrahedron Lett. 2010, 51, 4030-4032. [0135] (69) Meng, W.; Clegg, J. K.; Nitschke, J. R. Transformative Binding and Release of Gold Guests from a Self-Assembled Cu.sub.8L.sub.4 Tube. Angew. Chem. Int. Ed. 2012, 51, 1881-1884. [0136] (70) Meng, W.; League, A. B.; Ronson, T. K.; Clegg, J. K.; Isley, W. C.; Semrouni, D.; Gagliardi, L.; Cramer, C. J.; Nitschke, J. R. Empirical and Theoretical Insights into the Structural Features and Host-Guest Chemistry of M.sub.8L.sub.4 Tube Architectures. J. Am. Chem. Soc. 2014, 136, 3972-3980. [0137] (71) Christopherson, J. C.; Potts, K. P.; Bushuyev, O. S.; Topi?, F.; Huski?, I.; Rissanen, K.; Barrett, C. J.; Fri??i?, T. Assembly and Dichroism of a Four-Component Halogen-Bonded Metal-Organic Cocrystal Salt Solvate Involving Dicyanoaurate(I) Acceptors. Faraday Discuss. 2017, 203, 441-457. [0138] (72) Andersen, N. N.; Eriksen, K.; Lisbjerg, M.; Ottesen, M. E.; Milh?j, B. O.; Sauer, S. P. A.; Pittelkow, M. Entropy/Enthalpy Compensation in Anion Binding: Biotin[6]uril and Biotin-1-Sulfoxide[6]Uril Reveal Strong Solvent Dependency. J. Org. Chem. 2019, 84, 2577-2584. [0139] (73) Villiers, A. Sur La Fermentation de La F?cule Par L'action Du Ferment Butyrique. C.R. Acad. Sci. 1891, 112, 536. [0140] (74) Stoddart, J. F. A Century of Cyclodextrins. Carbohydr. Res. 1989, 192, 12-15. [0141] (75) Szejtli, J. Past, Present and Future of Cyclodextrin Research. Pure Appl. Chem. 2004, 76, 1825-1845. [0142] (76) Crini, G. Review: A History of Cyclodextrins. Chem. Rev. 2014, 114, 10940-10975. [0143] (77) Smaldone, R. A.; Forgan, R. S.; Furukawa, H.; Gassensmith, J. J.; Slawin, A. M. Z.; Yaghi, O. M.; Stoddart, J. F. Metal-Organic Frameworks from Edible Natural Products. Angew. Chem. Int. Ed. 2010, 49, 8630-8634. [0144] (78) Liu, Z.; Stoddart, J. F. Extended Metal-Carbohydrate Frameworks. Pure Appl. Chem. 2014, 86, 1323-1334. [0145] (79) Liu, Z.; Schneebeli, S. T.; Stoddart, J. F. Second-Sphere Coordination Revisited. Chimia (Aarau). 2014, 68, 315-320. [0146] (80) Harada, A.; Li, J.; Kamachi, M. The Molecular Necklace: A Rotaxane Containing Many Threaded a-Cyclodextrins. Nature 1992, 356, 325-327. [0147] (81) Noltemeyer, M.; Saenger, W. X-Ray Studies of Linear Polyiodide Chains in ?-Cyclodextrin Channels and a Model for the Starch-Iodine Complex. Nature 1976, 259, 629-632. [0148] (82) Noltemeyer, M.; Saenger, W. Topography of Cyclodextrin Inclusion Complexes. 12. Structural Chemistry of Linear.Alpha.-Cyclodextrin-Polyiodide Complexes. X-Ray Crystal Structures of (.Alpha.-Cyclodextrin)2.LiI.sub.3.I.sub.2.8H.sub.2O and (.Alpha.-Cyclodextrin).sub.2.Cd.sub.0.5).I.sub.5.27H.sub.2O. Models for the Blue. J. Am. Chem. Soc. 1980, 102, 2710-2722. [0149] (84) Spiwok, V. CH/? Interactions in Carbohydrate Recognition. Molecules 2017, 22, 1-11. [0150] (85) Nishio, M.; Umezawa, Y.; Fantini, J.; Weiss, M. S.; Chakrabarti, P. CH-? Hydrogen Bonds in Biological Macromolecules. Phys. Chem. Chem. Phys. 2014, 16, 12648-12683. [0151] (86) Nishio, M. The CH/? Hydrogen Bond in Chemistry. Conformation, Supramolecules, Optical Resolution and Interactions Involving Carbohydrates. Phys. Chem. Chem. Phys. 2011, 13, 13873-13900. [0152] (87) Ilioudis, C. A.; Tocher, D. A.; Steed, J. W. A Highly Efficient, Preorganized Macrobicyclic Receptor for Halides Based on CH . . . and NH . . . Anion Interactions. J. Am. Chem. Soc. 2004, 126, 12395-12402. [0153] (88) Vega, I. E. D.; Gale, P. A.; Light, M. E.; Loeb, S. J. NH vs. CH Hydrogen Bond Formation in Metal-Organic Anion Receptors Containing Pyrrolylpyridine Ligands. Chem. Commun. 2005, 39, 4913-4915. [0154] (89) Pedzisa, L.; Hay, B. P. Aliphatic CH . . . anion Hydrogen Bonds: Weak Contacts or Strong Interactions? J. Org. Chem. 2009, 74, 2554-2560. [0155] (90) Lisbjerg, M.; Valkenier, H.; Jessen, B. M.; Al-Kerdi, H.; Davis, A. P.; Pittelkow, M. Biotin[6]uril Esters: Chloride-Selective Transmembrane Anion Carriers Employing CH . . . Anion Interactions. J. Am. Chem. Soc. 2015, 137, 4948-4951. [0156] (91) Lefebvre, C.; Rubez, G.; Khartabil, H.; Boisson, J. C.; Contreras-Garc?a, J.; H?non, E. Accurately Extracting the Signature of Intermolecular Interactions Present in the NCI Plot of the Reduced Density Gradient Versus Electron Density. Phys. Chem. Chem. Phys. 2017, 19, 17928-17936. [0157] (92) Lu, T.; Chen, F. Multiwfn: A Multifunctional Wavefunction Analyzer. J. Comput. Chem. 2012, 33, 580-592. [0158] (97) Biedermann, F.; Nau, W. M.; Schneider, H. J. The Hydrophobic Effect Revisited-Studies with Supramolecular Complexes Imply High-Energy Water as a Noncovalent Driving Force. Angew. Chem. Int. Ed. 2014, 53, 11158-11171. [0159] (98) Snyder, P. W.; Lockett, M. R.; Moustakas, D. T.; Whitesides, G. M. Is It the Shape of the Cavity, or the Shape of the Water in the Cavity? Eur. Phys. J. Specia Top. 2014, 223, 853-891. [0160] (99) Hillyer, M. B.; Gibb, B. C. Molecular Shape and the Hydrophobic Effect. Annu. Rev. Phys. Chem. 2016, 67, 307-329. [0161] (100) Colquhoun, H. M.; Stoddart, J. F.; Williams, D. J. Second-Sphere CoordinationA Novel Role for Molecular Receptors. Angew. Chem. Int. Ed. 1986, 25, 487-507. [0162] (101) Alston, D. R.; Ashton, P. R.; Lilley, T. H.; Fraser Stoddart, J.; Zarzycki, R.; Slawin, A. M. Z.; Williams, D. J. Second-Sphere Coordination of Carboplatin and Rhodium Complexes by Cyclodextrins (Cyclomalto-Oigo-Saccharides). Carbohydr. Res. 1989, 192, 259-281. [0163] (102) Raymo, F. M.; Stoddart, J. F. Second-Sphere Coordination. Chem. Ber. 1996, 129, 981-990. [0164] (103) Alston, D. R.; Lilley, T. H.; Stoddart, J. F. The Binding of Cyclobutane-1,1-Dicarboxylatodiammineplatinum(II) by Alpha-Cyclodextrin in Aqueous Solution. J. Chem. Soc., Chem. Commun. 1985, 22, 1600-1602. [0165] (104) Alston, D. R.; Slawin, A. M. Z.; Stoddart, J. F.; Williams, D. J. The X-Ray Crystal Structure of a 1:1 Adduct between a-Cyclodextrin and Cyclobutane-1,1-Dicarboxylatodiammineplatinum(II). J. Chem.Soc., Chem. Commun. 1985, 22, 1602-1604. [0166] (105) Alston, D. R.; Slawin, A. M. Z.; Stoddart, J. F.; Williams, D. J. Cyclodextrins as Second Sphere Ligands for Transition Metal Complexes-The X-Ray Crystal Structure of [Rh(Cod)(NH.sub.3).sub.2.?-cyclodextrin][PF.sub.6].6H.sub.2O. Angew. Chem. Int. Ed. 1985, 24, 786-787. [0167] (106) Alston, D. R.; Slawin, A. M. Z.; Stoddart, J. F.; Williams, D. J.; Zarzycki, R. Second Sphere Coordination Adducts of Phosphane-Transition Metal Complexes with ?-Cyclodextrin and Its Methylated Derivative. Angew. Chem. Int. Ed. 1988, 27, 1184-1185.
EXAMPLES
[0168] The invention solves the commercial problems faced by today's gold-mining protocol, which requires the use of harsh conditions, including high temperature, high-pressure operation, and the use of toxic, corrosive and environmentally objectable chemicals, namely, NaCN and NaOH.
[0169] Molecular recognition of the Au(CN).sub.2.sup.? anion, a crucial intermediate in today's gold mining industry, by ?-cyclodextrin is demonstrated. Three X-ray single-crystal superstructures, KAu(CN).sub.2??-cyclodextrin, KAu(CN).sub.2?(?-cyclodextrin).sub.2 and KAg(CN).sub.2?(?-cyclodextrin).sub.2, demonstrate that the binding cavity of ?-cyclodextrin is a good fit for metal-coordination complexes, such as Au(CN).sub.2.sup.? and Ag(CN).sub.2.sup.? with linear geometries, while the K.sup.+ ions fulfil the role of linking ?-cyclodextrin tori together as a result of [K.sup.+ . . . O] ion-dipole interactions. A 1:1 binding stoichiometry between Au(CN).sub.2.sup.? and ?-cyclodextrin in aqueous solution, revealed by .sup.1H NMR titrations, has produced binding constants in the order of 10.sup.4 M.sup.?1. Isothermal calorimetry titrations indicate that this molecular recognition is driven by a favorable enthalpy change overcoming a small entropic penalty. The adduct formation of KAu(CN).sub.2??-cyclodextrin in aqueous solution is sustained by multiple [CH . . . ?] and [CH . . . Anion] interactions in addition to hydrophobic effects. The molecular recognition has also been investigated by DFT calculations, which suggest that the 2:1 binding stoichiometry between ?-cyclodextrin and Au(CN).sub.2.sup.? is favored in the presence of ethanol. This molecular recognition process between ?-cyclodextrin and KAu(CN).sub.2 can be applied to the stripping of gold from the surface of activated carbon at room temperature. Moreover, this stripping process is selective for Au(CN).sub.2.sup.? in the presence of Ag(CN).sub.2.sup.?, which has a lower binding affinity toward ?-cyclodextrin. This molecular recognition process allows for integration into commercial gold-mining protocols and lead to significantly reduced costs, energy consumption, and environmental impact.
Crystallographic Analyses
(1) Crystal Superstructure of KAu(CN).SUB.2.??-CD
[0170] (a) Method: Colorless block-like single crystals were obtained by slow evaporation of an aqueous solution (300 ?L) containing KAu(CN).sub.2 (8.9 mg) and ?-CD (30 mg) at room temperature for 30 days. A suitable crystal was selected, and the crystal was mounted on a MITIGEN holder with Paratone oil on a XtaLAB Synergy, Single source at home/near, HyPix diffractometer. The crystal was kept at 100.02(10) K during data collection. Using Olex2.sup.S1, the superstructure was solved with the ShelXT.sup.S2 structure solution program using Intrinsic Phasing and refined with the XL.sup.S3 refinement package using Least Squares minimization. [0171] (b) Crystal Parameters: Empirical formula=C.sub.38H.sub.74AuKN.sub.2O.sub.37, formula weight=1387.05, orthorhombic, space group P2.sub.12.sub.12.sub.1 (no. 19), a=13.99063(13), b=23.4405(2), c=51.2967(4) ?, V=16822.6(3) ?.sup.3, Z=12, T=100.02(10) K, ?(CuK?)=6.517 mm.sup.?1, D.sub.calc=1.643 g/mm.sup.3, 97178 reflections measured (6.548?2??160.584), 34431 unique (R.sub.int=0.0607, R.sub.sigma=0.0620) which were used in all calculations. The final R.sub.1 was 0.0588 (I>2?(I)) and wR.sub.2 was 0.1474 (all data). [0172] (c) Refinement Details: The enhanced rigid-bond restraint (SHELX keyword RIGU) was applied.sup.S4 globally.
[0173] (d) Solvent Treatment Details: The solvent masking procedure implemented in Olex2 was used to remove the electronic contribution of solvent molecules from the refinement. As the exact solvent content is unknown, only the atoms used in the refinement model are reported in the formula here. Total solvent-accessible volume/cell=889.1 ?.sup.3 [5.3%] Total electron count/cell=175.9.
TABLE-US-00002 TABLE 2 Distances between Au(CN).sub.2.sub.
(2) Crystal Superstructure of KAu(CN).SUB.2.??-CD
[0174] (a) Method: Colorless block-like single crystals were obtained by slow diffusion of EtOH into an aqueous solution (300 ?L) containing KAu(CN).sub.2 (8.9 mg) and ?-CD (30 mg) at room temperature for 14 days. A suitable crystal was selected, and the crystal was mounted on a MITIGEN holder with Paratone oil on a XtaLAB Synergy, Single source at offset/far, HyPix diffractometer. The crystal was kept at 100.0(2) K during data collection. Using Olex2.sup.S1, the superstructure was solved with the XT.sup.S2 structure solution program using Intrinsic Phasing and refined with the XL refinement package.sup.S3 using Least Squares minimization. [0175] (b) Crystal Parameters: Empirical formula=C.sub.39H.sub.74Au.sub.0.5K.sub.0.5NO.sub.35, formula weight=1235.02, triclinic, space group P
TABLE-US-00003 TABLE 3 Distances between Au(CN).sub.2.sub.
(3) Crystal Superstructure of KAg(CN).SUB.2.?2 ?-CD
[0178] Under the same conditions, we obtained the X-ray crystal superstructure of a 2:1 adduct between ?-CD and KAg(CN).sub.2. It is worth noting that KAg(CN).sub.2 is a byproduct in the cyanide-based, gold-mining process. The adduct has an identical superstructure with the 2:1 adduct between ?-CD and KAu(CN).sub.2. The two crystal superstructures are isostructural, suggesting the high similarity in superstructures and properties between these two 2:1 adducts. [0179] (a) Method: Colorless block-like single crystals were obtained by slow diffusion of EtOH into an aqueous solution (300 ?L) containing KAg(CN).sub.2 (6.2 mg) and ?-CD (30 mg) at room temperature during 14 days. A suitable crystal was selected, and the crystal was mounted on a MITIGEN holder with Paratone oil on a XtaLAB Synergy, Single source at offset/far, HyPix diffractometer. The crystal was kept at 99.98(17) K during data collection. Using Olex2.sup.S1, the superstructure was solved with the XT.sup.S2 structure solution program using Intrinsic Phasing and refined with the XL refinement package.sup.S3 using Least Squares minimization. [0180] (b) Crystal Parameters: Empirical formula=C.sub.78H.sub.148AgKN.sub.2O.sub.70, formula weight=2380.95, triclinic, space group P
TABLE-US-00004 TABLE 4 Distances between Ag(CN).sub.2.sub.
Computational Investigations
Visualization of Noncovalent Interactions
[0183] Independent Gradient Model (IGM) analysis is an approach.sup.S5 based on promolecular density (an electron density model prior to molecule formation) to identify and isolate intermolecular interactions. Strong polar attractions and van der Waals contacts are visualized as an iso-surface with blue and green color, respectively. Single crystal superstructures were used as input files. The binding surface was calculated by Multiwfn 3.6 program.sup.S6 through function 20 (visual study of weak interaction) and visualized by Chimera software..sup.S7
Binding Energy Analysis
[0184] The xyz coordinates for the single-point calculations were extracted from the X-ray single crystal data. All optimizations and single-point calculations were performed with density functional theory (DFT) in the Orca program.sup.S8 (version 4.1.2) using the Coulomb attenuated method (range-corrected) and hybrid Becke three-parameter Lee-Yang-Parr.sup.S9 (CAM-B3LYP) functional, the Ahlrich's double zeta basis set with a polarization function.sup.S10 Def2-SVP, and Grimme's third-generation dispersion with Beck Johnson damping (D3BJ). In order to speed up the DFT optimizations, the Coulomb integral and numerical chain-of-sphere integration for the HF exchanges.sup.S11,S12 (RIJCOSX) method was applied with the Def2/J auxiliary basiss.sup.S13 (AuxJ). The optimizations in a water continuum were performed with the Conductor like Polarizable Continuum Model.sup.S14 (CPCM) in Orca.
TABLE-US-00005 TABLE 5 Binding energies for optimizations in vacuum of (1:1) structures Electronic Binding Energy Entry Energy (DFT) (kcal mol.sup.?1) ?-CD ?3660.606331 NA Ag(CN).sub.2.sup.? ?332.4985083 NA Au(CN).sub.2.sup.? ?321.2813003 NA ?-CD-Ag(CN).sub.2.sup.? ?3993.162487 ?36.17 ?-CD-Au(CN).sub.2.sup.? ?3981.944433 ?35.64
TABLE-US-00006 TABLE 6 Binding energies for optimizations in water continuum of (1:1) structures Electronic Binding Energy Entry Energy (DFT) (kcal mol.sup.?1) ?-CD ?3660.647251 NA Ag(CN).sub.2.sup.? ?332.5811008 NA Au(CN).sub.2.sup.? ?321.3620598 NA ?-CD-Ag(CN).sub.2.sup.? ?3993.286396 ?36.42 ?-CD-Au(CN).sub.2.sup.? ?3982.061353 ?32.66
TABLE-US-00007 TABLE 7 Binding energies for (1:1) single crystal with Au(CN).sub.2.sup.? Electronic Binding Energy Entry Energy (DFT) (kcal mol.sup.?1) Au(CN).sub.2.sup.? ?321.2455053 NA K1.sup.+ ?599.6908053 NA A ?3659.75888 NA B ?3659.785735 NA C ?3659.808142 NA D ?3659.808339 NA E ?3659.785714 NA F ?3659.785733 NA G ?3659.808142 NA H ?3659.808266 NA I ?3659.785768 NA J ?3659.758687 NA K ?3659.758802 NA L ?3659.758991 NA M ?3659.758801 NA N ?3659.758686 NA O ?3659.758897 NA A . . . B ?7319.57024 ?16.08 A . . . C ?7319.567617 ?0.37 A . . . D ?7319.57169 ?2.81 A . . . E ?7319.561925 ?10.88 A . . . F ?7319.554659 ?6.30 A . . . G ?7319.567688 ?0.42 A . . . H ?7319.569673 ?1.59 A . . . I ?7319.56282 ?11.40 A . . . J ?7319.538412 ?13.08 A . . . K ?7319.53853 ?13.08 A . . . L ?7319.533808 ?10.00 A . . . M ?7319.557437 ?24.95 A . . . N ?7319.557323 ?24.95 A . . . O ?7319.533714 ?10.00 A . . . Au(CN).sub.2.sup.? ?3981.055943 ?32.35 (H.sub.2O).sub.2 (?-CD.sub.AHB).sub.3 ?11132.05969 NA K1.sup.+ (H.sub.2O).sub.2 ?11731.93202 ?113.91 (?-CD.sub.AHB).sub.3
[0185] The binding analysis of [?-CD . . . ?-CD] interaction is illustrated below. The excess of free water molecules around the cyclodextrins and not bound to K.sup.+ ions were removed. Only one potassium ion (labeled K1.sup.+) was selected to reduce computational cost.
TABLE-US-00008 TABLE 8 Selected binding energies for (1:2) single crystal adduct with Au(CN).sub.2.sup.? Electronic Binding Energy Entry Energy (DFT) (kcal mol.sup.?1) ?-CD (left side edge-to-edge) ?3659.805069 NA ?-CD (right side edge-to-edge) ?7319.650896 ?25.57 ?-CD . . . ?-CD (edge-to-edge) ?3659.786144 NA ?-CD . . . ?-CD (edge-to-edge) ?7319.675058 ?52.61 Au(CN).sub.2.sup.? ?321.278387 NA ?-CD ?3659.786129 NA Au(CN).sub.2.sup.? . . . ?-CD ?3981.13207 ?42.39 ?-CD . . . EtOH ?3814.569737 NA Au(CN).sub.2.sup.? . . . ?-CD . . . EtOH ?4135.948188 ?62.79 (?-CD).sub.2 ?7319.591187 NA Au(CN).sub.2.sup.? . . . (?-CD).sub.2 ?7640.996099 ?79.39 (?-CD).sub.2 . . . (EtOH).sub.2 ?7629.166154 NA Au(CN).sub.2.sup.? . . . (?-CD).sub.2 . . . (EtOH).sub.2 ?7950.635384 ?119.75
TABLE-US-00009 TABLE 9 Selected binding energies for (1:1) single crystal adduct with Ag(CN).sub.2.sup.? Electronic Binding Energy Entry Energy (DFT) (kcal mol.sup.?1) Ag(CN).sub.2.sup.? ?332.4620557 NA A ?3659.75888 NA A . . . Ag(CN).sub.2.sup.? ?3992.270807 ?31.29
TABLE-US-00010 TABLE 10 Selected binding energies for (1:2) single crystal adduct with Ag(CN).sub.2.sup.?. Electronic Binding Energy Entry Energy (DFT) (kcal mol.sup.?1) Ag(CN).sub.2.sup.? ?332.493334 NA ?-CD ?3659.780104 NA Ag(CN).sub.2.sup.? . . . ?-CD ?3992.323065 ?31.14 EtOH ?154.7830196 NA Ag(CN).sub.2.sup.? . . . ?-CD . . . EtOH ?4147.136268 ?50.08 (?-CD).sub.2 ?7319.534601 NA Ag(CN).sub.2.sup.? . . . (?-CD).sub.2 ?7652.147928 ?75.30 (?-CD).sub.2 . . . (EtOH).sub.2 ?7629.105661 NA Ag(CN).sub.2.sup.? . . . (?-CD).sub.2 . . . (EtOH).sub.2 ?7961.779314 ?113.15
Binding Studies Using NMR Spectroscopy
[0186] .sup.1H NMR Titration experiments in D.sub.2O were performed at 25? C. Aliquots from a stock solution containing the appropriate KAu(CN).sub.2 were added sequentially to an NMR tube containing the cyclodextrins, and a .sup.1H NMR spectrum was acquired after each addition. The titration isotherms were fitted to either 1:1 or 1:2 receptor-substrate binding model using Thordarson's equations.sup.S15 at http://app.supramolecular.org/bindfit/. All the titrations were independently duplicated (shown below is one set of titration isotherms) and all isotherm fittings were used to calculate the average K.sub.a with standard errors.
[0187] The titrations for ?- and ?-CD using Au(CN).sub.2.sup.? reveal (
[0188] 2:1 Binding models were used for the data fitting, resulting in K.sub.a values in the order of 10.sup.2 and 10.sup.1 M.sup.?1 for ?- and ?-CD, respectively, matching the results obtained from .sup.1H NMR titration experiments. The binding affinities of KAu(CN).sub.2 with ?- and ?-CD are much weaker and fit poorly to isotherms employing (
Binding Studies Using Isothermal Titration Calorimetry
[0189] Isothermal titration calorimetry (ITC) was performed by TA Nano Isothermal Titration calorimeter at 25? C. A Hastelloy cell was used with an active cell volume of 190 ?L. The stirring speed was set at 75 rpm. Receptor and substrate solutions were prepared in Milli-Q water and allowed to equilibrate overnight if necessary. In each titration experiment, 20-25 injections were performed with gradually decreased titration peaks until saturation is reached, at which point only heat of dilution was measured. The heat of dilution, when using ?-CD, was directly measured by titrating KAu(CN).sub.2 into a blank solution. After subtracting the heat of dilution, the resulting data were analyzed with NanoAnalyze software using either a 1:1 or a 1:2 receptor-substrate binding model and plotted by Origin Lab 8.6 software. All the titrations were independently duplicated. Shown below is one set of titration isotherms. All isotherm fittings were used to calculate the average K.sub.a and ?H with relevant standard errors.
Gold and Silver Stripping
Gold Adsorption on Activated Carbon
[0190] Activated carbon (10 g) was added to an aqueous solution (50 mL) of KAu(CN).sub.2 (150 mg, Au concentration: 2041 ppm), and the suspension was stirred at room temperature for 3 days. The activated carbon was filtrated and dried over the oven at 110? C. overnight. The remaining gold in the filtrate was analyzed by ICP, which revealed that the concentration of gold is less than 3 ppm, suggesting quantitative adsorption of Au on activated carbon. The activated carbon had a weight loss of 15% after drying under the same conditions, indicating 102 mg Au was adsorbed on 8.5 g activated carbon. The gold loading on activated carbon was thus calculated to be 12 mg/g.
Silver Adsorption on Activated Carbon
[0191] Activated carbon (10 g) was added to an aqueous solution (50 mL) of KAg(CN).sub.2 (150 mg, Ag concentration: 1613 ppm), and the suspension was stirred at room temperature for 3 days. The activated carbon was filtrated and dried in an oven at 110? C. overnight. The remaining gold in the filtrate was analyzed by ICP, which revealed that the concentration of gold is less than 3 ppm, suggesting quantitative adsorption of Ag on activated carbon. The activated carbon had a weight loss of 15% after drying under the same conditions, indicating 88 mg Ag was adsorbed on 8.5 g activated carbon. The silver loading on activated carbon was estimated to be 10 mg/g.
Gold and Silver Adsorption on Activated Carbon
[0192] Activated carbon (10 g) was added to an aqueous solution (50 mL) of KAu(CN).sub.2 (150 mg, Au concentration: 2041 ppm) and KAg(CN).sub.2 (150 mg, Ag concentration: 1613 ppm), and the suspension was stirred at room temperature for three days. The activated carbon was filtrated and dried in an oven at 110? C. overnight. The remaining gold and silver in the filtrate were analyzed by ICP, which revealed that the concentrations of gold and silver are less than 3 ppm, suggesting quantitative adsorption of Au and Ag on activated carbon. The activated carbon had a weight loss of 15% after drying under the same conditions, indicating 102 mg Au and 88 mg Ag were adsorbed on 8.5 g activated carbon. The gold and silver loading on activated carbon was estimated to be 12 and 10 mg/g, respectively.
Gold and/or Silver Stripping
[0193] Metal loaded activated carbon (50 mg, containing either 0.6 mg Au or 0.5 mg Ag) was added to an aqueous solution (5 mL) of ?-CD (0-10 w/v %, heat is applied to dissolve ?-CD when its concentration is >2% w/v %). The suspension was stirred for 30 min at room temperature, after which the activated carbon was separated by centrifuge. The supernatant was filtrated by a 0.45 ?m syringe filter, and the concentration of Au and Ag was analyzed by inductively coupled plasma mass spectrometry (ICP-MS). Each experiment was duplicated independently, and the average concentrations were presented with standard deviations. The same protocols were performed for gold stripping using ?-CD and selective gold string from the activated carbon loaded with both gold and silver.
ICP-MS Analysis
[0194] Quantification of gold (Au) and silver (Ag) was accomplished using ICP-MS of acidified samples. Specifically, samples (100 ?L) designated for Au analysis were digested in concentrated HNO.sub.3 (200 uL, 69%, Thermo Fisher Scientific, Waltham, MA, USA) and concentrated HCl (200 uL, 34%, Thermo Fisher Scientific, Waltham, MA, USA) at room temperature for 10 min in a ventilated hood. Cyanide test strips were used to ensure that no cyanide gas was evolving after this time, and ultra-pure H.sub.2O (18.2 M?.Math.cm) was added to produce a final solution of 2.0% HNO.sub.3 and 2.0% HCl (v/v) in a total sample volume of 10 mL. A quantitative standard was made using a 100 ?g/mL Au elemental standard (Inorganic Ventures, Christiansburg, VA, USA), which was used to create a 100 ng/g Au standard in 2.0% HNO.sub.3 and 2.0% HCl (v/v) in a total sample volume of 50 mL. A solution of 2.0% HNO.sub.3 and 2.0% HCl (v/v) was used as the calibration blank.
[0195] Samples designated for Ag analysis were digested in 200 uL concentrated trace nitric acid (>69%, Thermo Fisher Scientific, Waltham, MA, USA) at room temperature for 10 min in a ventilated hood. Cyanide test strips were used to ensure that no cyanide gas was evolving after this time, and ultra-pure H.sub.2O (18.2 M?.Math.cm) was added to produce a final solution of 2.0% HNO.sub.3 in a total sample volume of 10 mL. A quantitative standard was made using a 100 ?g/mL Ag elemental standard (Inorganic Ventures, Christiansburg, VA, USA), which was used to create a 100 ng/g Ag standard in 2.0% nitric acid in a total sample volume of 50 mL. A solution of 2.0% nitric acid was used as the calibration blank.
[0196] ICP-MS was performed on a computer-controlled (QTEGRA software) Thermo iCapQ ICP-MS (Thermo Fisher Scientific, Waltham, MA, USA) operating in STD mode and equipped with an ESI SC-2DX PrepFAST autosampler (Omaha, NE, USA). The internal standard was added inline using the prepFAST system and consisted of 1 ng/ml of a mixed element solution containing Bi, In, .sup.6Li, Sc, Tb, Y (IV-ICPMS-71D from Inorganic Ventures). Online dilution was also carried out by the prepFAST system and used to generate a calibration curve consisting of 100, 50, 10, 2 and 1 ppb Au or Ag. Each sample was acquired using 1 survey run (10 sweeps) and 3 main (peak jumping) runs (40 sweeps). The isotopes selected for analysis were .sup.107,109Ag or .sup.197Au and .sup.89Y, .sup.115In, .sup.159Tb, .sup.209Bi (chosen as internal standards for data interpolation and machine stability). Instrument performance is optimized daily through autotuning, followed by verification via a performance report (passing manufacturer specifications).
General Information
[0197] Commercially available solvents and chemicals were purchased from Sigma-Aldrich and Fisher Scientific and used without further purification unless otherwise stated. Nuclear magnetic resonance (NMR) spectra were recorded on a Bruker AVANCE III 600 MHz spectrometer. Chemical shifts are reported in ppm relative to the signals corresponding to the residual non-deuterated solvents. Single crystal data were obtained on a XtaLAB Synergy, Single source at offset/far, HyPix diffractometer. ICP-MS was performed on a computer-controlled (QTEGRA software) Thermo iCapQ ICP-MS (Thermo Fisher Scientific, Waltham, MA, USA) operating in STD mode and equipped with an ESI SC-2DX PrepFAST autosampler (Omaha, NE, USA). Detailed experimental procedures are provided in the appropriate sections that follow this one. Activated carbon (Part number: 05105, Lot code: 1136095) were purchased from Fluka with the following specifications (Table 11):
TABLE-US-00011 TABLE 11 Specifications of the activated carbon. Loss on drying (110? C.) <15% Co <0.001% Ash (600? C.) <0.1% Cr <0.001% Iodine-adsorption >70 ml/g Cu <0.001% (0.05 mol I.sub.2/I) Methylene blue- >12 ml/0.1 g Fe <0.03% adsorption (0.15% sol.) Soluble material in <0.2% K <0.02% ethanol Soluble material in HCl .sup.<1% Mg <0.02% Water-soluble matter <0.5% Mn <0.005% Chloride (Cl) <0.5% Na <0.05% Sulfate (SO.sub.4) <0.5% Ni <0.001% Ca <0.1% Pb <0.001% Cd <0.001% Zn <0.001%
REFERENCES
[0198] (S1) Dolomanov, O. V; Bourhis, L. J.; Gildea, R. J.; Howard, J. A. K.; Puschmann, H. OLEX2: A Complete Structure Solution, Refinement and Analysis Program. J. Appl. Crystallogr. 2009, 42, 339-341. [0199] (S2) Sheldrick, G. M. SHELXT-Integrated Space-Group and Crystal-Structure Determination. Acta Crystallogr. Sect. A 2015, 71, 3-8. [0200] (S3) Sheldrick, G. M. A Short History of SHELX. Acta Crystallogr. Sect. A 2008, 64, 112-122. [0201] (S4) Thorn, A.; Dittrich, B.; Sheldrick, G. M. Enhanced Rigid-Bond Restraints. Acta Crystallogr. Sect. A 2012, 68, 448-451. [0202] (S5) Lefebvre, C.; Rubez, G.; Khartabil, H.; Boisson, J. C.; Contreras-Garc?a, J.; H?non, E. Accurately Extracting The Signature of Intermolecular Interactions Present in The NCI Plot of The Reduced Density Gradient Versus Electron Density. Phys. Chem. Chem. Phys. 2017, 19, 17928-17936. [0203] (S6) Lu, T.; Chen, F. Multiwfn: A Multifunctional Wavefunction Analyzer. J. Comput. Chem. 2012, 33, 580-592. [0204] (S7) Pettersen, E. F.; Goddard, T. D.; Huang, C. C.; Couch, G. S.; Greenblatt, D. M.; Meng, E. C.; Ferrin, T. E. UCSF ChimeraA Visualization System for Exploratory Research and Analysis. J. Comput. Chem. 2004, 25, 1605-1612. [0205] (S8) Neese, F. The ORCA Program System. WIREs Comput. Mol. Sci. 2012, 2, 73-78. [0206] (S9) Becke, A. D. Density-functional Thermochemistry. III. The Role of Exact Exchange. J. Chem. Phys. 1993, 98, 5648-5652. [0207] (S10) Weigend, F.; Ahlrichs, R. Balanced Basis Sets of Split Valence{,} Triple Zeta Valence and Quadruple Zeta Valence Quality for H to Rn: Design and Assessment of Accuracy. Phys. Chem. Chem. Phys. 2005, 7, 3297-3305. [0208] (S11) Neese, F. An Improvement of the Resolution of the Identity Approximation for the Formation of the Coulomb Matrix. J. Comput. Chem. 2003, 24, 1740-1747. [0209] (S12) Izs?k, R.; Neese, F. An Overlap Fitted Chain of Spheres Exchange Method. J. Chem. Phys. 2011, 135, 144105. [0210] (S13) Stoychev, G. L.; Auer, A. A.; Neese, F. Automatic Generation of Auxiliary Basis Sets. J. Chem. Theory Comput. 2017, 13, 554-562. [0211] (S14) Barone, V.; Cossi, M. Quantum Calculation of Molecular Energies and Energy Gradients in Solution by a Conductor Solvent Model. J. Phys. Chem. A 1998, 102, 1995-2001. [0212] (S15) Thordarson, P. Determining Association Constants from Titration Experiments in Supramolecular Chemistry. Chem. Soc. Rev. 2011, 40, 1305-1323.