Optical sheet for backlight unit and backlight unit
10754083 ยท 2020-08-25
Assignee
Inventors
- Kenichi HARADA (Tokyo, JP)
- Yoshitada NAMIKAWA (Tokyo, JP)
- Tadayoshi FUKUDA (Tokyo, JP)
- Yuki Matsuno (Tokyo, JP)
Cpc classification
G02B6/0038
PHYSICS
G02B6/0081
PHYSICS
B32B27/304
PERFORMING OPERATIONS; TRANSPORTING
B32B2255/10
PERFORMING OPERATIONS; TRANSPORTING
B32B2457/202
PERFORMING OPERATIONS; TRANSPORTING
B32B27/302
PERFORMING OPERATIONS; TRANSPORTING
B32B23/04
PERFORMING OPERATIONS; TRANSPORTING
B32B27/308
PERFORMING OPERATIONS; TRANSPORTING
G02B6/0036
PHYSICS
B32B2307/546
PERFORMING OPERATIONS; TRANSPORTING
B32B3/30
PERFORMING OPERATIONS; TRANSPORTING
B32B27/20
PERFORMING OPERATIONS; TRANSPORTING
G02B6/005
PHYSICS
International classification
Abstract
An optical sheet for a backlight unit for guiding toward a front face side rays of light emitted by an LED light source. The optical sheet includes one or more resin layers. Ultrafine grooves oriented in specific directions are provided on a front face side or a back face side of at least one resin layer of the one or more resin layers. An average number of the ultrafine grooves per unit length in a direction perpendicular to an average orientation of the ultrafine grooves is preferably no less than 10/mm and no greater than 10,000/mm. A face of the at least one resin layer provided with the ultrafine grooves preferably has an arithmetic average roughness (Ra) in a direction perpendicular to an orientation of the ultrafine grooves being no less than 0.01 m and no greater than 5 m. Ultrafine grooves preferably constitute a diffraction grating.
Claims
1. A light diffusion sheet for a backlight unit for a liquid crystal display device, the light diffusion sheet being for guiding toward a front face side rays of light emitted by an LED light source, wherein the light diffusion sheet comprises a plurality of resin layers, the plurality of resin layers comprising: a bass film; a light diffusion layer that is laminated on a front face side of the base film and comprises beads and a binder for the beads; and a protective layer laminated on a back face side of the base film, and ultrafine grooves oriented in specific directions that transmit rays of light in a width direction to inhibit creation of hot spots are provided on a front face side or a back face side of at least one resin layer of the plurality of resin layers.
2. The light diffusion sheet for a backlight unit according to claim 1, wherein an average number of the ultrafine grooves per unit length in a direction perpendicular to an average orientation of the ultrafine grooves is no less than 10/mm and no greater than 10,000/mm.
3. The light diffusion sheet for a backlight unit according to claim 1, wherein a face of the at least one resin layer provided with the ultrafine grooves has an arithmetic average roughness (Ra) in a direction perpendicular to an orientation of the ultrafine grooves being no less than 0.01 m and no greater than 5 m.
4. The light diffusion sheet for a backlight unit according to claim 1, wherein the ultrafine grooves constitute a diffraction grating.
5. The light diffusion sheet for a backlight unit according to claim 1, wherein the ultrafine grooves are provided on a back face side of the protective layer.
6. The light diffusion sheet for a backlight unit according to claim 1, further comprising a functional layer comprising projections and recesses provided on a front face thereof.
7. The light diffusion sheet for a backlight unit according to claim 1, wherein one resin layer of the one or more resin layers comprises ultrafine projections and recesses on a front face thereof, and the ultrafine grooves are provided on a face of the one resin layer provided with the ultrafine projections and recesses.
8. A backlight unit for a liquid crystal display device comprising: a light guide film or a light guide plate for guiding toward a front face side thereof rays of light having entered from an end face side thereof; one or more LED light sources that are disposed on the end face side of the light guide film or the light guide plate and are for emitting rays of light to an end face of the light guide film or the light guide plate; and the light diffusion sheet according to claim 1 overlaid on the front face side of the light guide film or the light guide plate.
9. The backlight unit for a liquid crystal display device according to claim 8, wherein the light diffusion sheet is overlaid directly on a front face of the light guide film or the light guide plate.
10. The backlight unit according to claim 8, wherein in a planar view, an average orientation of the ultrafine grooves of the light diffusion sheet with respect to an average direction of the rays of light emitted by the one or more LED light sources and incident on the light guide film or the light guide plate is directed at an angle within a range of45 to 45.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1)
(2)
(3)
(4)
(5)
(6)
(7)
(8)
(9)
(10)
(11)
(12)
(13)
(14)
(15)
(16)
(17)
(18)
(19)
(20)
(21)
(22)
(23)
DESCRIPTION OF EMBODIMENTS
(24) Hereinafter, embodiments of the present invention will be described in detail with appropriate references to the drawings.
(25) First Embodiment
(26) Backlight Unit
(27) The backlight unit of the liquid crystal display device illustrated in
(28) Underlayer Light Diffusion Sheet
(29) As illustrated in
(30) Base Film
(31) The base film 11 is a resin layer containing a synthetic resin as a principal component. Since the base film 11 needs to transmit rays of light, the base film 11 is formed from a transparent synthetic resin, particularly a colorless and transparent synthetic resin as a principal component. The principal component of the base film 11 is not particularly limited, and examples thereof include polyethylene terephthalate, polyethylene naphthalate, acrylic resins, polycarbonates, polystyrenes, polyolefins, cellulose acetate, weather resistant vinyl chlorides, and the like. Among these, polyethylene terephthalate having excellent transparency and high strength are preferred, and polyethylene terephthalate with improved deflection performance is particularly preferred.
(32) The lower limit of an average thickness of the base film 11 is preferably 10 m, more preferably 35 m, and still more preferably 50 m. The upper limit of the average thickness of the base film 11 is preferably 500 m, more preferably 250 m, and still more preferably 188 m. In the case where the average thickness of the base film 11 is less than the lower limit, a curl may occur in the formation of the light diffusion layer 12 by coating. In the case where the average thickness of the base film 11 is less than the lower limit, deflections may be developed. Conversely, in the case where the average thickness of the base film 11 is greater than the upper limit, the luminance of the liquid crystal display device may be reduced, and a requirement for a reduction in the thickness of the liquid crystal display device may not be satisfied. It is to be noted that the term average thickness as referred to herein means a value obtained by averaging the thicknesses measured at randomly chosen 10 points.
(33) Light Diffusion Layer
(34) The light diffusion layer 12 is a resin layer containing a synthetic resin as a principal component. The light diffusion layer 12 constitutes the frontmost face of the underlayer light diffusion sheet 4. The light diffusion layer 12 contains the beads 14 in a dispersion state with a substantially uniform density. The beads 14 are surrounded by the binder 15. The light diffusion layer 12 in which the beads 14 are contained in a dispersion state is capable of diffusing, substantially uniformly, rays of light transmitted from the back face side to the front face side. In addition, due to the beads 14, ultrafine projections and recesses are provided substantially uniformly on the front face of the light diffusion layer 12, and the individual protruding portions and the individual recessed portions of the ultrafine projections and recesses are lens-shaped. The light diffusion layer 12 performs, owing to a lens-like effect of the ultrafine projections and recesses, a superior light diffusion function, and thus has, owing to its light diffusion function, both the function of refracting transmitted rays of light toward the normal direction and the function of condensing the transmitted rays of light macroscopically into the normal direction.
(35) The beads 14 are resin particles having the property of diffusing rays of light. Examples of the principal component of the beads 14 include acrylic resins, acrylonitrile resins, polyurethane, polyvinyl chloride, polystyrene, polyamide, polyacrylonitrile, and the like. Of these, highly transparent acrylic resins are preferred, and polymethyl methacrylate (PMMA) is particularly preferred.
(36) The shape of the beads 14 is not particularly limited, and may be for example, spherical, cubic, needle-like, rod-like, spindle-like, plate-like, scale-like, fiber-like, etc. In particular, spherical beads are preferred in light of superior light diffusibility.
(37) The lower limit of the mean particle diameter of the beads 14 is preferably 1 m, more preferably 2 m, and still more preferably 5 m. The upper limit of the mean particle diameter of the beads 14 is preferably 50 m, more preferably 20 m, and still more preferably 15 m. In the case where the mean particle diameter of the beads 14 is less than the lower limit, the projections and recessions of the front surface of the light diffusion layer 12 are reduced, and the light diffusion sheet may not have the required light diffusibility. Conversely, in the case where the mean particle diameter of the beads 14 is greater than the upper limit, the thickness of the underlayer light diffusion sheet 4 may be increased, and it may be difficult to diffuse rays of light uniformly.
(38) The lower limit of the content of the beads 14 (the content thereof on solid content basis with respect to 100 parts by mass of polymer components in a polymer composition which is a material for forming the binder 15) is preferably 10 parts by mass, more preferably 20 parts by mass, and still more preferably 50 parts by mass. The upper limit of the content of the beads 14 is preferably 500 parts by mass, more preferably 300 parts by mass, and still more preferably 200 parts by mass. In the case where the content of the light diffusing agent 14 is less than the lower limit, the light diffusibility may be insufficient. Conversely, in the case where the content of the beads 14 is greater than the upper limit, the beads 14 may not be fixed properly by the binder 15.
(39) The binder 15 is prepared by hardening (through crosslinking, etc.) a polymer composition containing a base polymer. The binder 15 allows the beads 14 to be arranged and fixed with a substantially uniform density on the entire front face of the base film 11. It is to be noted that, for example, a fine inorganic filler, a curing agent, a plasticizer, a dispersant, various types of levelling agents, an antistatic agent, an ultraviolet ray-absorbing agent, an anti-oxidizing agent, a viscosity modifier, a lubricant, a light stabilizer, and the like may be further blended in the polymer composition for forming the binder 15, as needed.
(40) Protective Layer
(41) The protective layer 13 is a resin layer containing a synthetic resin as a principal component. The ultrafine grooves 16 are provided on the back face of the protective layer 13. The ultrafine grooves 16 preferably constitute the diffraction grating. The ultrafine grooves 16 are preferably formed as hairline stripes. For the backlight unit including the underlayer light diffusion sheet 4, in the case where the ultrafine grooves 16 are provided on the back face side of the protective layer 13 of the underlayer light diffusion sheet 4, the rays of light passing through the regions defined by the ultrafine grooves 16 are likely to be transmitted sufficiently in the width direction of the ultrafine grooves, owing to a difference in refractive index between the protective layer 13 and an air layer present on the back face side of the protective layer 13. Since the ultrafine grooves 16 are provided on the back face side of the protective layer 13 of the underlayer light diffusion sheet 4, the front face of the light guide film 1 partially abuts the back face of the protective layer 13. This enables prevention of the sticking of the underlayer light diffusion sheet 4 to the light guide film 1. In the case where the ultrafine grooves 16 constitute the diffraction grating, a diffraction phenomenon occurs, where the rays of light passing through the regions defined by the ultrafine grooves 16 have a certain optical path difference. Owing to the diffraction phenomenon, the underlayer light diffusion sheet 4 is likely to inhibit the creation of hot spots easily and reliably.
(42) As illustrated in
(43) In a planar view, the average orientation of the ultrafine grooves 16 with respect to the average direction of the rays of light emitted by the LED light sources 2 and incident on the light guide film 1 is preferably directed at an angle within a range of 45 to 45, more preferably directed at an angle within a range of 15 to 15, and still more preferably directed at an angle of 0. In the case where the average orientation falls outside the above range, it may be difficult to transmit the rays of light in the direction perpendicular to and the direction parallel to the direction of the rays of light emitted by the LED light sources 2 and in the horizontal direction. In the case where the average orientation falls within the range, the backlight unit is likely to inhibit the creation of hot spots easily and reliably.
(44) As illustrated in
(45) The lower limit of an average width L.sub.2 of the ultrafine grooves 16 is preferably 10 nm, more preferably 50 nm, and still more preferably 100 nm. The upper limit of the average width L.sub.2 of the ultrafine grooves 16 is preferably 40 m, more preferably 30 m, still more preferably 20 m, and particularly preferably 10 m. In the case where the average width L.sub.2 of the large ultrafine grooves 16 is less than the lower limit, formability of the ultrafine grooves 16 may deteriorate. Conversely, in the case where the average width L.sub.2 of the ultrafine grooves 16 is greater than the upper limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. It is preferred that the width L.sub.2 of each of the ultrafine grooves 16 varies randomly within the above range, along the longitudinal direction. In the case where each of the ultrafine grooves 16 is formed such that the width L.sub.2 thereof varies randomly within the above range, prevention of moire caused by interference with other members (e.g., prism sheets, liquid crystal cells, etc.) having a cyclic pitch is enabled. Also, prevention of regularly occurring color separation is enabled, and in turn, prevention of iridescent unevenness is enabled. It is to be noted that the term average width of the ultrafine grooves as referred to herein means a value obtained by averaging widths measured at randomly chosen points except for the longitudinal ends, of randomly chosen 20 ultrafine grooves on the average interface of the resin layer.
(46) The upper limit of the average pitch of the ultrafine grooves 16 is preferably 10 nm, more preferably 50 nm, and still more preferably 100 nm. The upper limit of the average pitch of the ultrafine grooves 16 is preferably 40 m, more preferably 30 m, still more preferably 20 m, and particularly preferably 10 m. In the case where the average pitch of the ultrafine grooves 16 is less than the lower limit, formability of the ultrafine grooves 16 may deteriorate. Conversely, in the case where the average pitch of the ultrafine grooves 16 is greater than the upper limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. It is to be noted that the term average pitch of the ultrafine grooves as referred to herein means a value obtained by averaging the pitches of randomly chosen 10 ultrafine grooves that are adjacent to each other in the direction perpendicular to the average orientation of the ultrafine grooves.
(47) The upper limit of the standard deviation of the pitches of the ultrafine grooves 16 is preferably 10 m, more preferably 9 m, and still more preferably 7 m. In the case where the standard deviation of the pitches of the ultrafine grooves 16 is greater than the upper limit, the ultrafine grooves 16 may be irregular in pitch, and thus, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased evenly. The lower limit of the standard deviation of the pitches of the ultrafine grooves 16 may be, for example, 4 m, in light of ease in arranging the ultrafine grooves 16 in comparatively random directions. It is to be noted that the term standard deviation of the pitches of the ultrafine grooves as referred to herein means a standard deviation of the pitches of randomly chosen 20 ultrafine grooves.
(48) It is preferred that the average width L.sub.2 and the average pitch of the ultrafine grooves 16 respectively fall within the above ranges. Due to the average width L.sub.2 and the average pitch of the ultrafine grooves 16 respectively falling within the above ranges, the underlayer light diffusion sheet 4 is capable of sufficiently increasing the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 easily and reliably.
(49) The lower limit of the average number of the ultrafine grooves 16 per unit length in the direction perpendicular to the average orientation of the ultrafine grooves 16 is preferably 10/mm, more preferably 50/mm, and still more preferably 100/mm. The upper limit of the average number is preferably 10,000/mm, more preferably 5,000/mm, and still more preferably 1,000/mm. In the case where the average number is less than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. Conversely, in the case where the average number is greater than the upper limit, formability of the ultrafine grooves 16 may deteriorate.
(50) The lower limit of an average depth D.sub.1 of the ultrafine grooves 16 is preferably 10 nm, more preferably 500 nm, still more preferably 1 m, and particularly preferably 2 m. The upper limit of the average depth D.sub.1 of the ultrafine grooves 16 is preferably 30 m, more preferably 10 m, still more preferably 5 m, and particularly preferably 3 m. In the case where the average depth D.sub.1 of the ultrafine grooves 16 is less than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. Conversely, in the case where the average depth D.sub.1 of the ultrafine grooves 16 is greater than the upper limit, the strength of the protective layer 13 may be decreased. It is to be noted that the term average depth of the ultrafine grooves as referred to herein means a value obtained by averaging the depths of randomly chosen 20 ultrafine grooves, each depth being the distance between the average interface of the resin layer and the bottom of the ultrafine groove concerned.
(51) The upper limit of the standard deviation of the depths of the ultrafine grooves 16 is preferably 4 m, more preferably 3 m, and still more preferably 2.5 m. In the case where the standard deviation of the depths of the ultrafine grooves 16 is greater than the upper limit, the ultrafine grooves 16 may be irregular in depth, and thus, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased evenly. The lower limit of the standard deviation of the depths of the ultrafine grooves 16 is not particularly limited, and may be, for example, 0.3 m. It is to be noted that the term standard deviation of the depths of the ultrafine grooves as referred to herein means a standard deviation of the depths of randomly chosen 20 ultrafine grooves.
(52) The lower limit of the arithmetic average roughness (Ra), in the direction parallel to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 0.005 m, more preferably 0.05 m, and still more preferably 0.1 m. The upper limit of the arithmetic average roughness (Ra), in the direction parallel to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 1.5 m, more preferably 1.2 m, and still more preferably 1 m. In the case where the arithmetic average roughness (Ra) is less than the lower limit, the effect of inhibiting the creation of hot spots may be insufficient. Conversely, in the case where the arithmetic average roughness (Ra) is greater than the upper limit, the amount of rays of light transmitted in the direction parallel to the orientation of the ultrafine grooves 16 may be great with respect to the amount of rays of light transmitted in the width direction of the ultrafine grooves 16.
(53) The lower limit of the arithmetic average roughness (Ra), in the direction perpendicular to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 0.01 m, more preferably 0.1 m, and still more preferably 0.5 m. The upper limit of the arithmetic average roughness (Ra), in the direction perpendicular to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 5 m, more preferably 2 m, still more preferably 1.7 m, and particularly preferably 1.5 m. In the case where the arithmetic average roughness (Ra) is less than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. Conversely, in the case where the arithmetic average roughness (Ra) is greater than the upper limit, it may be difficult to regulate the angles at which the rays of light are emitted.
(54) For the arithmetic average roughness (Ra) of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16, it is preferred that the average roughness (Ra) in the direction parallel to the orientation of the ultrafine grooves 16 and the arithmetic average roughness (Ra) in the direction perpendicular to the orientation of the ultrafine grooves 16 respectively fall within the above ranges. In the case where the arithmetic average roughness (Ra) in the direction parallel to the orientation of the ultrafine grooves 16 and the arithmetic average roughness (Ra) in the direction perpendicular to the ultrafine grooves 16 respectively fall within the above ranges, the underlayer light diffusion sheet 4 is likely to sufficiently increase the amount of rays of light transmitted in the width direction of the ultrafine grooves 16, thus inhibiting the creation of hot spots easily and reliably.
(55) For the face (back face) of the protective layer 13 provided with the ultrafine grooves 16, the lower limit of the difference between the arithmetic average roughness (Ra) in the direction perpendicular to the orientation of the ultrafine grooves 16 and the arithmetic average roughness (Ra) in the direction parallel to the orientation of the ultrafine grooves 16 is preferably 0.5 m, more preferably 0.7 m, and still more preferably 1 m. In the case where the difference in the arithmetic average roughness (Ra) is greater than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 is increased, and thus, the lack in uniformity of luminance of the liquid crystal display device is likely to be reduced easily and reliably. The upper limit of the difference in arithmetic average roughness (Ra) may be, for example, 1.9 m.
(56) The lower limit of the maximum height (Ry) of the face (back face), in the direction parallel to the orientation of the ultrafine grooves 16, of the protective layer 13 provided with the ultrafine grooves 16 is preferably 0.1 m, more preferably 1 m, and still more preferably 1.5 m. The upper limit of the maximum height (Ry), in the direction parallel to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 3 m, more preferably 2.5 m, and still more preferably 2 m. In the case where the maximum height (Ry) is less than the lower limit, the effect of inhibiting the creation of hot spots may be insufficient. Conversely, in the case where the maximum height (Ry) is greater than the upper limit, the amount of rays of light transmitted in the direction parallel to the orientation of the ultrafine grooves 16 may be great with respect to the amount of rays of light transmitted in the width direction of the ultrafine grooves 16. The term maximum height (Ry) as referred to herein means a value determined in accordance with JIS-B0601: 1994, with a cut-off c of 0.8 mm and an evaluation length of 4 mm.
(57) The lower limit of the maximum height (Ry) of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 in the direction perpendicular to the orientation of the ultrafine grooves 16 is preferably 4 m, more preferably 5 m, and still more preferably 6 m. The upper limit of the maximum height (Ry) of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 in the direction perpendicular to the orientation of the ultrafine grooves 16 is preferably 12 m, more preferably 10 m, and still more preferably 9 m. In the case where the maximum height (Ry) is less than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. Conversely, in the case where the maximum height (Ry) is greater than the upper limit, it may be difficult to regulate the angles at which the rays of light are emitted.
(58) For the face (back face) of the protective layer 13 provided with the ultrafine grooves 16, the lower limit of the difference between the maximum height (Ry) in the direction perpendicular to the orientation of the ultrafine grooves 16 and the maximum height (Ry) in the direction parallel to the orientation of the ultrafine grooves 16 is preferably 4 m, more preferably 5 m, and still more preferably 6 m. In the case where the difference in the maximum height (Ry) is greater than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 is increased, and thus, the lack in uniformity of luminance of the liquid crystal display device is likely to be reduced easily and reliably. The upper limit of the difference in maximum height (Ry) may be, for example, 11 m.
(59) The lower limit of the ten-point mean roughness (Rz), in the direction parallel to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 0.1 m, more preferably 0.5 m, and still more preferably 1 m. The upper limit of the ten-point mean roughness (Rz), in the direction parallel to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 2.5 m, more preferably 2 m, and still more preferably 1.5 m. In the case where the ten-point mean roughness (Rz) is less than the lower limit, the effect of inhibiting the creation of hot spots may be insufficient. Conversely, in the case where the ten-point mean roughness (Rz) is greater than the upper limit, the amount of rays of light transmitted in the direction parallel to the orientation of the ultrafine grooves 16 may be great with respect to the amount of rays of light transmitted in the width direction of the ultrafine grooves 16. The term ten-point mean roughness (Rz) as referred to herein means a value determined in accordance with JIS-B0601: 1994, with a cut-off c of 0.8 mm and an evaluation length of 4 mm.
(60) The lower limit of the ten-point mean roughness (Rz), in the direction perpendicular to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 4 m, more preferably 5 m, and still more preferably 6 m. The upper limit of the ten-point mean roughness (Rz), in the direction perpendicular to the orientation of the ultrafine grooves 16, of the face of the protective layer 13 provided with the ultrafine grooves 16 is preferably 10 m, more preferably 8 m, and still more preferably 7 m. In the case where the ten-point mean roughness (Rz) is less than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. Conversely, in the case where the ten-point mean roughness (Rz) is greater than the upper limit, it may be difficult to regulate the angles at which the rays of light are emitted.
(61) For the face (back face) of the protective layer 13 provided with the ultrafine grooves 16, the lower limit of the difference between the ten-point mean roughness (Rz) in the direction perpendicular to the orientation of the ultrafine grooves 16 and the ten-point mean roughness (Rz) in the direction parallel to the orientation of the ultrafine grooves 16 is preferably 3 m, more preferably 4 m, and still more preferably 4.5 m. In the case where the difference in the ten-point mean roughness (Rz) is greater than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 is increased, and thus, the lack in uniformity of luminance of the liquid crystal display device is likely to be reduced easily and reliably. The upper limit of the difference in ten-point mean roughness (Rz) may be, for example, 9 m.
(62) The lower limit of the root mean square slope (Rq), in the direction parallel to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 0.05, more preferably 0.2, still more preferably 0.25, and particularly preferably 0.3. The upper limit of the root mean square slope (Rq), in the direction parallel to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 0.5, more preferably 0.45, and still more preferably 0.4. In the case where the root mean square slope (Rq) is less than the lower limit, the effect of inhibiting the creation of hot spots may be insufficient. Conversely, in the case where the root mean square slope (Rq) is greater than the upper limit, the amount of rays of light transmitted in the direction parallel to the orientation of the ultrafine grooves 16 may be great with respect to the amount of rays of light transmitted in the width direction of the ultrafine grooves 16. The term root mean square slope (Rq) as referred to herein means a value determined in accordance with JIS-B0601: 2001.
(63) The lower limit of the root mean square slope (Rq), in the direction perpendicular to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 0.5, more preferably 0.7, and still more preferably 1. The upper limit of the root mean square slope (Rq), in the direction perpendicular to the orientation of the ultrafine grooves 16, of the face (back face) of the protective layer 13 provided with the ultrafine grooves 16 is preferably 2.5, more preferably 2, and still more preferably 1.8. In the case where the root mean square slope (Rq) is less than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 may not be increased sufficiently. Conversely, in the case where the root mean square slope (Rq) is greater than the upper limit, it may be difficult to regulate the angles at which the rays of light are emitted.
(64) For the face (back face) of the protective layer 13 provided with the ultrafine grooves 16, the lower limit of the difference between the root mean square slope (Rq) in the direction perpendicular to the orientation of the ultrafine grooves 16 and the root mean square slope (Rq) in the direction parallel to the orientation of the ultrafine grooves 16 is preferably 0.5, more preferably 0.7, and still more preferably 1. In the case where the difference in the root mean square slope (Rq) is greater than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 16 is increased, and thus, the lack in uniformity of luminance of the liquid crystal display device is likely to be reduced easily and reliably. The upper limit of the difference in root mean square slope (Rq) may be, for example, 2.2.
(65) The principal component of the protective layer 13 is exemplified by a polycarbonate, an acrylic resin, a urethane resin, an acrylic-urethane copolymer, polyethylene terephthalate, polyethylene naphthalate, a polystyrene, a methyl (meth)acrylate-styrene copolymer, a polyolefin, a cycloolefin polymer, a cycloolefin copolymer, cellulose acetate, a weather resistant vinyl chloride, an active energy ray-curable resin, and the like. Of these, an acrylic resin is preferred, which increases the strength of the back face of the underlayer light diffusion sheet 4 and is likely to prevent generation of scratches on the back face.
(66) The lower limit of the average thickness of the protective layer 13 is preferably 1 m, and more preferably 5 m. The upper limit of the average thickness of the protective layer 13 is preferably 50 m, and more preferably 10 m. In the case where the average thickness of the protective layer 13 is less than the lower limit, generation of scratches on the back face of the underlayer light diffusion sheet 4 may not be prevented properly. Conversely, in the case where the average thickness of the protective layer 13 is greater than the upper limit, the luminance of the liquid crystal display device may be reduced.
(67) The lower limit of the refractive index of the protective layer 13 is preferably 1.36, more preferably 1.4, and still more preferably 1.43. The upper limit of the refractive index of the protective layer 23 is preferably 1.7, more preferably 1.5, and still more preferably 1.49. In the case where the refractive index of the protective layer 13 falls within the above range, the amount of the rays of light transmitted in the width direction of the ultrafine grooves 16 is increased, owing to the difference in refractive index between the protective layer 13 and the air layer present on the back face side of the protective layer 13, and thus, the lack in uniformity of luminance of the liquid crystal display device is likely to be reduced easily and reliably.
(68) Prism Sheet
(69) Each of the first prism sheet 5 and the second prism sheet 6 includes a substrate layer and a row of projections including protruding-streak prism portions laminated on the front face of the substrate layer. Since the substrate layer and the protruding-streak prism portions need to transmit rays of light, each of the substrate layer and the protruding-streak prism portions is a resin layer containing a transparent synthetic resin, particularly a colorless and transparent synthetic resin as a principal component. The ridge line direction of the protruding-streak prism portions of the first prism sheet 5 is substantially orthogonal to the ridge line direction of the protruding-streak prism portions of the second prism sheet 6.
(70) The lower limit of the thickness of each of the first prism sheet 5 and the second prism sheet 6 (the height from the back face of the substrate layer to the vertex of each protruding-streak prism portion) is preferably 50 m, and more preferably 100 m. The upper limit of the thickness of each of the first prism sheet 5 and the second prism sheet 6 is preferably 200 m, and more preferably 180 m. The lower limit of the pitch of the protruding-streak prism portions of each of the first prism sheet 5 and the second prism sheet 6 is preferably 30 m, and more preferably 40 m. The upper limit of the pitch of the protruding-streak prism portions of each of the first prism sheet 5 and the second prism sheet 6 is preferably 100 m, and more preferably 60 m. The vertex angle of each protruding-streak prism portion is preferably no less than 85 and no greater than 95. The lower limit of the refractive index of each of the first prism sheet 5 and the second prism sheet 6 is preferably 1.5, and more preferably 1.55. The upper limit of the refractive index of each of the first prism sheet 5 and the second prism sheet 6 is preferably 1.7. It is to be noted that the term refractive index of the prism sheet as referred to herein means the refractive index of the protruding-streak prism portions.
(71) Upper-Layer Light Diffusion Sheet
(72) The upper-layer light diffusion sheet 7 includes: a base film; a light diffusion layer that is laminated on a front face side of the base film and contains beads and a binder for the beads; and a protective layer laminated on a back face side of the base film. The upper-layer light diffusion sheet 7 has a three-layer structure including the base film, the light diffusion layer laminated directly on the front face of the base film, and the protective layer laminated directly on the back face of the base film. The upper-layer light diffusion sheet 7 does not include layers other than the base film, the light diffusion layer and the protective layer. The upper-layer light diffusion sheet 7 is formed into a rectangular shape in a planar view.
(73) Each of the base film, the light diffusion layer and the protective layer of the upper-layer light diffusion sheet 7 is a resin layer containing a synthetic resin as a principal component. The base film of the upper-layer light diffusion sheet 7 may have a configuration similar to that of the base film 11 of the underlayer light diffusion sheet 4. The protective layer of the upper-layer light diffusion sheet 7 may have a configuration similar to that of the protective layer 13 of the underlayer light diffusion sheet 4, except that the protective layer is not provided with ultrafine grooves. Meanwhile, the light diffusibility of the light diffusion layer of the upper-layer light diffusion sheet 7 does not need to be as high as that of the light diffusion layer 12 of the underlayer light diffusion sheet 4. Thus, the lower limit of the content of a light diffusing agent is preferably 5 parts by mass and more preferably 10 parts by mass, whereas the upper limit thereof is preferably 40 parts by mass and more preferably 30 parts by mass.
(74) Light Guide Film
(75) The light guide film 1 allows the rays of light incident on its end face to exit from its front face substantially uniformly. The light guide film 1 is formed into a plate-like shape (non-wedge shape) that is substantially rectangular in a planar view and has a substantially uniform thickness. The light guide film 1 includes, on the back face thereof, recessed portions 17 falling toward the front face side. In addition, the light guide film 1 includes, on the back face thereof, sticking preventive portions. Specifically, the light guide film 1 includes, as the sticking preventive portions, raised portions 18 provided to surround the recessed portions 17, and protruding toward the back face side. The raised portions 18 adjoin the recessed portions 17, with the forming face of each recessed portion 17 being continuous with the inner lateral face of each surrounding raised portion 18. The light guide film 1 is a resin layer containing a synthetic resin as a principal component.
(76) The lower limit of the average thickness of the light guide film 1 is preferably 100 m, more preferably 150 m, and still more preferably 200 m. The upper limit of the average thickness of the light guide film 1 is preferably 600 m, more preferably 580 m, and still more preferably 550 m. In the case where the average thickness of the light guide film 1 is less than the lower limit, the strength of the light guide film 1 may be insufficient, and the rays of light from the LED light sources 2 may not be allowed to enter the light guide film 1 sufficiently. Conversely, in the case where the average thickness of the light guide film 1 is greater than the upper limit, the requirement for a reduction in the thickness of the backlight unit of this embodiment may not be satisfied.
(77) The recessed portions 17 function as a light scattering portion for scattering incident light toward the front face side. Each recessed portion 17 is formed into a substantially circular shape in a planar view. Furthermore, each recessed portions 17 is formed such that the diameter thereof gradually decreases toward the front face side. The shape of each recessed portion 17 is not particularly limited, and may be hemispherical, semielliptical, conical, frustoconical, or the like. Of these, the shape of each recessed portion 17 is preferably hemispherical or semielliptical. In the case where the recessed portions 17 each have a hemispherical or semielliptical shape, the formability of the recessed portions 17 may be improved, and additionally, rays of light incident on the recessed portions 17 can be favorably scattered.
(78) The raised portions 18 are formed on the back face of the light guide film 1, so as to be continuous with the surface perpendicular to the thickness direction of the light guide film 1. Specifically, the raised portions 18 are formed so as to be continuous with the flat surface of the back face of the light guide film 1. The raised portions 18 are formed to be substantially annular in a planar view so as to surround the recessed portions 17. In the case where the raised portions 18 are formed to be substantially annular in a planar view so as to surround the recessed portions 17, the light guide film 1 is capable of easily and reliably preventing the recessed portions 17 and the vicinity of the recessed portions 17 from sticking to the reflection sheet 8 disposed on the back face side of the light guide film 1.
(79) The light guide film 1 has flexibility. Owing to the flexibility, the light guide film 1 is capable of inhibiting generation of scratches on the reflection sheet 8 disposed on the back face side of the light guide film 1. Since the light guide film 1 needs to transmit rays of light, the light guide film 1 is formed to be transparent, in particular, colorless and transparent.
(80) The principal component of the light guide film 1 is exemplified by a polycarbonate, an acrylic resin, polyethylene terephthalate, polyethylene naphthalate, a polystyrene, a methyl (meth)acrylate-styrene copolymer, a polyolefin, a cycloolefin polymer, a cycloolefin copolymer, cellulose acetate, a weather resistant vinyl chloride, an active energy ray-curable resin, and the like. Of these, polycarbonate or an acrylic resin is preferred as the principal component of the light guide film 1. In the case where the light guide sheet 1 contains a polycarbonate, which has superior transparency and a high refractive index, as a principal component, the total reflection is likely to occur on the front and back faces of the light guide film 1, whereby rays of light can be efficiently transmitted. In addition, owing to the heat resistance of the polycarbonate, the light guide film 1 is less prone to, for example, degradation caused by heat of the LED light sources 2. Furthermore, a polycarbonate is less water-absorbent than acrylic resins and the like, and is thus superior in dimension accuracy to the acrylic resins and the like. Therefore, due to containing a polycarbonate as the principal component, the light guide film 1 is capable of inhibiting degradation over time. On the other hand, since the acrylic resins have a higher degree of transparency, a loss of rays of light in the light guide film 1 can be reduced.
(81) LED Light Sources
(82) The LED light sources 2 are disposed along the end face of the light guide film 1. Each of the LED light sources 2 is disposed in such a manner that a light emission surface thereof faces (or abuts) the end face of the light guide film 1.
(83) Reflection Sheet
(84) The reflection sheet 8 includes a resin layer containing a synthetic resin as a principal component. The reflection sheet 8 may be configured either as a white resin layer in which a filler is dispersed in a base resin such as a polyester, or as a mirror sheet obtained by vapor deposition of a metal such as aluminum and silver on the front face of a resin layer formed from a polyester or the like to enhance regular reflection properties.
(85) Function of Reducing Lack in Uniformity of Luminance
(86) With reference to
(87) With reference to
(88) Advantages
(89) In the case where the optical sheet for a backlight unit of this embodiment (the underlayer light diffusion sheet 4) is included in a backlight unit equipped with LEDs serving as the light sources, the optical sheet is capable of inhibiting the creation of hot spots. Although the reason for this effect is not necessarily clarified, it is presumed that the rays of light passing through regions defined by the ultrafine grooves 16, which are provided on the resin layer of the optical sheet for a backlight unit and are oriented in the specific directions, are transmitted in the width direction of the ultrafine grooves 16, and that the inhibition of the creation of hot spots is enabled even when highly directive rays of light are emitted by the LEDs.
(90) The optical sheet for a backlight unit of this embodiment (the underlayer light diffusion sheet 4) includes the base film 11, the light diffusion layer 12 that is laminated on the front face side of the base film 11 and contains the beads 14 and the binder 15 for the beads 14, and the protective layer 13 laminated on the back face side of the base film 11, and thus, rays of light diffused substantially uniformly over the entire face are likely to be emitted.
(91) The backlight unit, which includes the optical sheet for a backlight unit (the underlayer light diffusion sheet 4), is capable of inhibiting the creation of hot spots as described above.
(92) The backlight unit of this embodiment, in which the optical sheet of this embodiment (the underlayer light diffusion sheet 4) is overlaid directly on the front face of the light guide film 1, is capable of sufficiently inhibiting the creation of hot spots.
(93) Method for Producing Underlayer Light Diffusion Sheet
(94) A method for producing the underlayer light diffusion sheet 4 of this embodiment includes: forming a sheet body which is to serve as the base film 11 (base film-forming step); laminating the protective layer 13 on one face side of the sheet body (protective layer-laminating step); and laminating the light diffusion layer 12 on the other face side of the sheet body (light diffusion layer-laminating step).
(95) Base Film-Forming Step
(96) Although the base film-forming step is not particularly limited, the step may be exemplified by a process of forming the sheet body by subjecting a molten thermoplastic resin to extrusion molding using a T die, and subsequently drawing the extrusion-molded article in both a layer longitudinal direction and a layer width direction. Well-known extrusion molding processes employing the T die may include, for example, a polishing roll process and a chill roll process. In addition, drawing processing of the extrusion-molded article may be exemplified by a biaxial drawing process for tubular films, a biaxial drawing process for flat films, and the like.
(97) Protective Layer-Laminating Step
(98) The protective layer-laminating step is exemplified by a process in which a coating liquid containing materials for forming the protective layer is applied to one face side of the sheet body formed in the base film-forming step, and then the shape of the ultrafine grooves 16 is transferred to one face side of a coating film obtained by the application of the coating liquid, by using a mold having on the surface thereof a reversal shape of the ultrafine grooves 16. The process for applying the coating liquid is not particularly limited, and may be exemplified by spin coating, spray coating, slide coating, dip coating, bar coating, roll coating, screen printing, or the like. As the mold, a metal roller or a metal plate having on the surface thereof a reversal shape of the ultrafine grooves 16 may be used. In the protective layer-laminating step, the coating film may be dried as needed. In the protective layer-laminating step, the coating film having the shape of ultrafine grooves 16 transferred to the one face side thereof may be hardened by heating, ultraviolet irradiation, or the like. The base film-forming step and the protective layer-laminating step may be simultaneously performed by using a coextrusion molding process. In the protective layer-laminating step, a sheet body obtained by hardening the material for forming the protective layer is laminated on one face side of the base film, and then, the ultrafine grooves 16 may be formed on one face of the sheet body by laser processing, filing, or the like, or the ultrafine grooves 16 may be formed on the sheet body by a photolithography process and an etching process.
(99) Light Diffusion Layer-Laminating Step
(100) The light diffusion layer-laminating step is exemplified by a process in which a coating liquid containing the beads 14 and a binder composition is applied onto the other face side of the sheet body, and then the coating liquid thus applied is dried and hardened.
(101) The method for producing the underlayer light diffusion sheet of this embodiment may further include a surface treatment process in which the surface of sheet body on which the light diffusion layer is to be laminated is subjected to, before undergoing the light diffusion layer-laminating step, a corona discharge treatment, an ozone treatment, a low-temperature plasma treatment, a glow discharge treatment, an oxidization treatment, a primer coating treatment, an undercoat treatment, an anchor coating treatment, or the like.
(102) Advantages
(103) The method for producing the underlayer light diffusion sheet of this embodiment allows easy and reliable production of the underlayer light diffusion sheet 4 that is capable of inhibiting the creation of hot spots as described above.
(104) Second Embodiment
(105) Underlayer Light Diffusion Sheet
(106) In place of the underlayer light diffusion sheet 4 illustrated in
(107) Base Film
(108) The base film 25 is a resin layer containing a synthetic resin as a principal component. Since the base film 25 needs to transmit rays of light, the base film 25 is formed from a transparent synthetic resin, particularly a colorless and transparent synthetic resin as a principal component. The principal component of the base film 25 is not particularly limited, and is exemplified by the synthetic resins similar to those exemplified in relation to the principal component of the base film 11 of the underlayer light diffusion sheet 4 illustrated in
(109) Ultrafine grooves 27 are provided on a back face of the protective layer 25. The ultrafine grooves 27 preferably constitute the diffraction grating. The ultrafine grooves 27 are preferably formed as hairline stripes.
(110) The ultrafine grooves 27 are formed substantially evenly (with a substantially uniform density) on the entire back face of the base film 25. The ultrafine grooves 27 each have a substantially U-shaped cross section (in other words, the ultrafine grooves 27 each do not have a triangular cross section). The longitudinal direction of the ultrafine grooves 27 is parallel to one end of the back face of the base film 25. Specifically, the longitudinal direction of the ultrafine grooves 27 is aligned with the average direction of the rays of light emitted by the LED light sources. Furthermore, the ultrafine grooves 27 are irregular in orientation. Although the ultrafine grooves 27 are preferably provided discretely for the purpose of regulating the diffusion direction of the rays of light, some of the ultrafine grooves 27 may intersect with each other. The average orientation, the average length in the longitudinal direction, the average width, the average pitch, the standard deviation of the pitches, the number per unit length, the average depth, and the standard deviation of the depths of the ultrafine grooves 27 may be similar to those of the ultrafine grooves 16 of the underlayer light diffusion sheet 4 illustrated in
(111) The lower limit of the refractive index of the base film 25 is preferably 1.51, more preferably 1.53, and still more preferably 1.55. The upper limit of the refractive index of the base film 25 is preferably 1.7, more preferably 1.67, and still more preferably 1.65. In the case where there is a large difference between the refractive index of the base film 25 and the refractive index of another layer (the protective layer 26) laminated on the face (back face) of the base film 25 provided with the ultrafine grooves 27, the underlayer light diffusion sheet 24 of this embodiment is more likely to increase the amount of rays of light transmitted in the width direction of the ultrafine grooves 27. In this respect, in the case where the refractive index of the base film 25 is less than the lower limit, the difference in refractive index between the base film 25 and the protective layer 26 is not sufficiently large, leading to a failure to sufficiently increase the amount of rays of light transmitted in the width direction of the ultrafine grooves 27. Conversely, in the case where the refractive index of the base film 25 is greater than the upper limit, there may be a restriction on resins that can be used for the base film 25. The term refractive index as referred to herein means a refractive index for light having a wavelength of 589.3 nm (sodium D-line), which is an average of three measurements conducted at a temperature of 23 C., using a plate-like test piece of 70 mm on each side and 2 mm in thickness.
(112) The lower limit of the difference between the refractive index of the base film 25 and the refractive index of the other layer (the protective layer 26) laminated on the face (back face) of the base film 25 provided with the ultrafine grooves 27 is preferably 0.01, more preferably 0.05, and still more preferably 0.07. In the case where the difference in refractive index is less than the lower limit, the amount of rays of light transmitted in the width direction of the ultrafine grooves 27 may not be increased sufficiently. The upper limit of the difference in refractive index may be, for example, 0.15.
(113) Protective Layer
(114) The protective layer 26 is a resin layer containing a synthetic resin as a principal component. The principal component of the protective layer 26 is exemplified by the synthetic resins exemplified in relation to the principal component of the protective layer 26 of the underlayer light diffusion sheet 4 illustrated in
(115) The lower limit of the refractive index of the protective layer 26 is preferably 1.36, more preferably 1.4, and still more preferably 1.43. The upper limit of the refractive index of the protective layer 26 is preferably 1.51, more preferably 1.5, and still more preferably 1.49. In the case where the refractive index of the protective layer 26 is less than the lower limit, there may be a restriction on resins that can be used for the protective layer 26. Conversely, in the case where the refractive index of the protective layer 26 is greater than the upper limit, the difference in refractive index between the base film 25 and the protective layer 26 is not sufficiently large, leading to a failure to sufficiently increase the amount of rays of light transmitted in the width direction of the ultrafine grooves 27.
(116) Method for Producing Underlayer Light Diffusion Sheet
(117) A method for producing the underlayer light diffusion sheet 24 of this embodiment includes: forming a sheet body which is to serve as the base film 25 (base film-forming step); laminating the protective layer 26 on one face side of the sheet body (protective layer-laminating step); and laminating the light diffusion layer 12 on the other face side of the sheet body (light diffusion layer-laminating step). The light diffusion layer-laminating step according to the method for producing the underlayer light diffusion sheet 24 is similar to the light diffusion layer-laminating step of the underlayer light diffusion sheet 4 illustrated in
(118) Base Film-Forming Step
(119) The base film-forming step is exemplified by an extrusion molding process in which a molten thermoplastic resin is subjected to extrusion molding using a T die, and then the shape of the ultrafine grooves 27 is transferred to one face side of the extrusion-molded article by using a mold having on the surface thereof a reversal shape of the ultrafine grooves 27. In the base film-forming step, the extrusion-molded article may be drawn in both a layer longitudinal direction and a layer width direction. Well-known extrusion molding processes employing the T die may include, for example, a polishing roll process and a chill roll process. As the mold, a metal roller or a metal plate having on the surface thereof a reversal shape of the ultrafine grooves 27 may be used. Furthermore, drawing processing of the extrusion-molded article may be exemplified by a biaxial drawing process for tubular films, a biaxial drawing process for flat films, and the like. In the base film-forming step, the extrusion-molded article is formed, and then, the ultrafine grooves 27 may be formed on one face of the extrusion-molded article by laser processing, filing, or the like, or the ultrafine grooves 27 may be formed on the sheet body by a photolithography process and an etching process.
(120) Protective Layer-Laminating Step
(121) The protective layer-laminating step is exemplified by a coating process in which a coating liquid containing materials for forming the protective layer is applied to one face side of the sheet body formed in the base film-forming step, and then the coating liquid is dried and hardened. The process for applying the coating liquid is exemplified by the processes exemplified in relation to the protective layer-laminating step of the underlayer light diffusion sheet 4 illustrated in
(122) Advantages
(123) The underlayer light diffusion sheet 24 of this embodiment is capable of inhibiting the creation of hot spots. The underlayer light diffusion sheet 34 is likely to allow emission of rays of light diffused substantially uniformly over the entire face thereof.
(124) The method for producing the underlayer light diffusion sheet of this embodiment allows easy and reliable production of the underlayer light diffusion sheet 24 that is capable of inhibiting the creation of hot spots.
(125) Third Embodiment
(126) Underlayer Light Diffusion Sheet
(127) In place of the underlayer light diffusion sheets 4 and 24 illustrated in
(128) Base Film
(129) The base film 35 is a resin layer containing a synthetic resin as a principal component. Since the base film 35 needs to transmit rays of light, the base film 35 is formed from a transparent synthetic resin, particularly a colorless and transparent synthetic resin as a principal component. The principal component of the base film 35 is not particularly limited, and is exemplified by the synthetic resins similar to those exemplified in relation to the principal component of the base film 11 of the underlayer light diffusion sheet 4 illustrated in
(130) Ultrafine grooves 40 are provided on the front face of the base film 35. The ultrafine grooves 40 preferably constitute the diffraction grating. A specific constitution of the ultrafine grooves 40 may be similar to that of the ultrafine grooves 27 of the underlayer light diffusion sheet 24 illustrated in
(131) The refractive index of the base film 35 may be similar to that of the base film 25 of the underlayer light diffusion sheet 24 illustrated in
(132) Light Diffusion Layer
(133) The light diffusion layer 36 is a resin layer containing a synthetic resin as a principal component. The light diffusion layer 36 constitutes the frontmost face of the underlayer light diffusion sheet 34. The light diffusion layer 36 contains the beads 38 in a dispersion state with a substantially uniform density. The beads 38 are surrounded by the binder 39. The light diffusion layer 36 in which the beads 38 are contained in a dispersion state is capable of diffusing, substantially uniformly, rays of light transmitted from the back face side to the front face side. In addition, due to the beads 38, ultrafine projections and recesses are provided substantially uniformly on the front face of the light diffusion layer 36, and the individual protruding portions and the individual recessed portions of the ultrafine projections and recesses are lens-shaped. The light diffusion layer 36 performs, owing to a lens-like effect of the ultrafine projections and recesses, a superior light diffusion function, and thus has, owing to its light diffusion function, both the function of refracting transmitted rays of light toward the normal direction and the function of condensing the transmitted rays of light macroscopically into the normal direction.
(134) The principal component of the beads 38 may be similar to that of the beads 14 of the underlayer light diffusion sheet 4 illustrated in
(135) The binder 39 is prepared by hardening (through crosslinking, etc.) a polymer composition containing a base polymer. The binder 39 allows the beads 38 to be arranged and fixed with a substantially uniform density on the entire front face of the base film 35.
(136) The lower limit of the refractive index of the binder 39 is preferably 1.36, more preferably 1.4, and still more preferably 1.43. The upper limit of the refractive index of the binder 39 is preferably 1.7, more preferably 1.6, still more preferably 1.55, and even more preferably 1.49. In the case where the refractive index of the protective layer 39 is less than the lower limit, there may be a restriction on resins that can be used for the binder 39. Conversely, in the case where the refractive index of the protective layer 39 is greater than the upper limit, the difference in refractive index between the base film 25 and the binder 39 is not sufficiently large, leading to a failure to sufficiently increase the amount of rays of light transmitted in the width direction of the ultrafine grooves 40.
(137) Protective Layer
(138) The protective layer 37 is a resin layer containing a synthetic resin as a principal component. The back face of the protective layer 37 is formed into a flat surface. The principal component of the protective layer 37 is exemplified by the synthetic resins exemplified in relation to the principal component of the protective layer 13 of the underlayer light diffusion sheet 4 illustrated in
(139) Method for Producing Underlayer Light Diffusion Sheet
(140) A method for producing the underlayer light diffusion sheet 34 of this embodiment includes: forming a sheet body which is to serve as the base film 35 (base film-forming step); laminating the protective layer 37 on one face side of the sheet body (protective layer-laminating step); and laminating the light diffusion layer 36 on the other face side of the sheet body (light diffusion layer-laminating step). The method for producing this underlayer light diffusion sheet of this embodiment may be similar to the method for producing the underlayer light diffusion sheet 24 illustrated in
(141) Advantages
(142) The underlayer light diffusion sheet 34 of this embodiment is capable of inhibiting the creation of hot spots. The underlayer light diffusion sheet 34 is likely to allow emission of rays of light diffused substantially uniformly over the entire face thereof.
(143) The method for producing the underlayer light diffusion sheet of this embodiment allows easy and reliable production of the underlayer light diffusion sheet 34 that is capable of inhibiting the creation of hot spots.
(144) Fourth Embodiment
(145) Underlayer Light Diffusion Sheet
(146) In place of the underlayer light diffusion sheets 4, 24 and 34 illustrated in
(147) Light Diffusion Layer
(148) The light diffusion layer 45 is a resin layer containing a synthetic resin as a principal component. The light diffusion layer 45 constitutes the frontmost face of the underlayer light diffusion sheet 44. The light diffusion layer 45 contains the beads 46 in a dispersion state with a substantially uniform density. The beads 46 are surrounded by the binder 47. The light diffusion layer 45 in which the beads 46 are contained in a dispersion state is capable of diffusing, substantially uniformly, rays of light transmitted from the back face side to the front face side. In addition, due to the beads 46, ultrafine projections and recesses are provided substantially uniformly on the front face of the light diffusion layer 45. The light diffusion layer 45 performs, owing to a lens-like effect of the ultrafine projections and recesses, a superior light diffusion function, and thus has, owing to its light diffusion function, both the function of refracting transmitted rays of light toward the normal direction and the function of condensing the transmitted rays of light macroscopically into the normal direction. Furthermore, ultrafine grooves 48 are provided on the front face of the light diffusion layer 45. In other words, the ultrafine grooves 48 of this embodiment are provided on the face of the underlayer light diffusion sheet 44 provided with the ultrafine projections and recesses. In the case the ultrafine grooves 48 are provided on the face of the underlayer light diffusion sheet 44 provided with the ultrafine projections and recesses, the ultrafine grooves 48 enable transmission of the rays of light in the width direction of the ultrafine grooves 48, and the ultrafine projections and recesses enable diffusion of the rays of light. This enables improvements in the effects of, for example, preventing moire, preventing color separation, and expanding the viewing angle. The ultrafine grooves 48 preferably constitute the diffraction grating. A specific constitution of the ultrafine grooves 48 may be similar to that of the ultrafine grooves 16 of the underlayer light diffusion sheet 4 illustrated in
(149) The principal component of the beads 46 may be similar to that of the beads 14 of the underlayer light diffusion sheet 4 illustrated in
(150) Method for Producing Underlayer Light Diffusion Sheet
(151) A method for producing the underlayer light diffusion sheet 44 of this embodiment includes: forming a sheet body which is to serve as the base film 11 (base film-forming step); laminating the protective layer 37 on one face side of the sheet body (protective layer-laminating step); and laminating the light diffusion layer 45 on the other face side of the sheet body (light diffusion layer-laminating step). The base film-forming step according to the method for producing the underlayer light diffusion sheet 44 is similar to the base film-forming step of the underlayer light diffusion sheet 4 illustrated in
(152) Light Diffusion Layer-Laminating Step
(153) The light diffusion layer-laminating step is exemplified by a process in which a coating liquid containing the beads 46 and a binder composition is applied to the other face side of the sheet body formed in the base film-forming step, and then the shape of the ultrafine grooves 48 is transferred to one face side of a coating film obtained by the application of the coating liquid, by using a mold having on the surface thereof a reversal shape of the ultrafine grooves 48. In the light diffusion layer-laminating step, a mold having on the surface thereof the shape of ultrafine projections and recesses in addition to the reversal shape of the ultrafine grooves 48 may be used. In the case where the mold having on the surface thereof the shape of the ultrafine projections and recesses is used in the light diffusion layer-laminating step, ultrafine projections and recesses are formed on the front face of the light diffusion layer 45. The light diffusion layer 45 performs, owing to a lens-like effect of the ultrafine projections and recesses, a superior light diffusion function, and thus has, owing to its light diffusion function, both the function of refracting transmitted rays of light toward the normal direction and the function of condensing the transmitted rays of light macroscopically into the normal direction. The process for applying the coating liquid is exemplified by the processes exemplified in relation to the protective layer-laminating step of the underlayer light diffusion sheet 4 illustrated in
(154) Advantages
(155) The underlayer light diffusion sheet 44 of this embodiment is capable of inhibiting the creation of hot spots. The underlayer light diffusion sheet 44 is likely to allow emission of rays of light diffused substantially uniformly over the entire face thereof. In general, the diffraction effect of the backlight unit associated with the diffraction grating increasingly becomes noticeable as the distance between the LED light sources and the diffraction grating increases. In the case where the diffraction grating is formed on the front face of the light diffusion layer 9 constituting the frontmost face of the underlayer light diffusion sheet 44, a reduction in the lack in uniformity of luminance of the liquid crystal display device is enabled more reliably.
(156) The method for producing the underlayer light diffusion sheet of this embodiment allows easy and reliable production of the underlayer light diffusion sheet 44 of this embodiment that is capable of inhibiting the creation of hot spots.
(157) Fifth Embodiment
(158) Underlayer Light Diffusion Sheet
(159) In place of the underlayer light diffusion sheets 4, 24, 34, and 44 illustrated in
(160) Method for Producing Underlayer Light Diffusion Sheet
(161) A method for producing the underlayer light diffusion sheet 54 of this embodiment includes: forming a sheet body which is to serve as the base film 35 (base film-forming step); laminating the protective layer 13 on one face side of the sheet body (protective layer-laminating step); and laminating the light diffusion layer 36 on the other face side of the sheet body (light diffusion layer-laminating step). The base film-forming step and the light diffusion layer-laminating step according to the method for producing the underlayer light diffusion sheet 54 may be similar to the base film-forming step and the light diffusion layer-laminating step of the underlayer light diffusion sheet 34 illustrated in
(162) Advantages
(163) The underlayer light diffusion sheet 54 of this embodiment, in which ultrafine grooves are provided on the two resin layers, is capable of inhibiting the creation of hot spots more reliably. The underlayer light diffusion sheet 54 is likely to allow emission of rays of light diffused substantially uniformly over the entire face thereof.
(164) Sixth Embodiment
(165) Underlayer Light Diffusion Sheet
(166) In place of the underlayer light diffusion sheets 4, 24, 34, 44 and 54 illustrated in
(167) Method for Producing Underlayer Light Diffusion Sheet
(168) A method for producing the underlayer light diffusion sheet 64 of this embodiment includes: forming a sheet body which is to serve as the base film 35 (base film-forming step); laminating the protective layer 13 on one face side of the sheet body (protective layer-laminating step); and laminating the light diffusion layer 45 on the other face side of the sheet body (light diffusion layer-laminating step). The base film-forming step according to the method for producing the underlayer light diffusion sheet 64 may be similar to the base film-forming step of the underlayer light diffusion sheet 34 illustrated in
(169) Advantages
(170) The underlayer light diffusion sheet 64 of this embodiment, in which ultrafine grooves are provided on the three resin layers, is capable of inhibiting the creation of hot spots more reliably. The underlayer light diffusion sheet 64 is likely to allow emission of rays of light diffused substantially uniformly over the entire face thereof.
(171) Seventh Embodiment
(172) Underlayer Light Diffusion Sheet
(173) In place of the underlayer light diffusion sheets 4, 24, 34, 44, 54 and 64 illustrated in
(174) Protective Layer
(175) The protective layer 75 is a resin layer containing a synthetic resin as a principal component. The principal component of the protective layer 75 is exemplified by the synthetic resins exemplified in relation to the principal component of the protective layer 13 of the underlayer light diffusion sheet 4 illustrated in
(176) Ultrafine grooves 76 are provided on the back face of the protective layer 75. The ultrafine grooves 76 are provided on a certain region extending from one end to the other end of the back face of the protective layer 75. Specifically, the ultrafine grooves 76 are provided on the certain region extending from the edge opposed to the LED light sources to the other end of the protective layer 75 in a planar view. The region of the back face of the protective layer 75 that is not provided with the ultrafine grooves 76 constitutes a flat surface. The ultrafine grooves 76 each have a substantially U-shaped cross section (in other words, the ultrafine grooves 76 each do not have a triangular cross section). The ultrafine grooves 76 preferably constitute the diffraction grating.
(177) The lower limit of the ratio (L.sub.4/L.sub.3) of a length L.sub.4 between one end and the other end of the region provided with the ultrafine grooves 76, to a length L.sub.3 between one end and the other end of the back face of the protective layer 75, is preferably 0.15, more preferably 0.2, and still more preferably 0.25. The upper limit of the length ratio (L.sub.4/L.sub.3) is preferably 0.5, more preferably 0.45, and still more preferably 0.4. In the case where the length ratio (L.sub.4/L.sub.3) is less than the lower limit, it may be difficult to entirely inhibit the creation of hot spots. Conversely, in the case where the length ratio (L.sub.4/L.sub.3) is greater than the upper limit, it may be difficult to transmit, in the width direction of the ultrafine grooves 76, ray of light in the region other than the hot spots.
(178) The longitudinal direction of the ultrafine grooves 76 is parallel to one end of the back face of the protective layer 75. Specifically, the longitudinal direction of the ultrafine grooves 76 is aligned with the average direction of the rays of light emitted by the LED light sources. Furthermore, the ultrafine grooves 76 are irregular in orientation. Although the ultrafine grooves 76 are preferably provided discretely for the purpose of regulating the diffusion direction of the rays of light, some of the ultrafine grooves 76 may intersect with each other. The average orientation, the average length in the longitudinal direction, the average width, the average pitch, the standard deviation of the pitches, the average number per unit length, the average depth, and the standard deviation of the depths of the ultrafine grooves 76 may be similar to those of the ultrafine grooves 16 of the underlayer light diffusion sheet 4 illustrated in
(179) Method for Producing Underlayer Light Diffusion Sheet
(180) The method for producing the underlayer light diffusion sheet 74 of this embodiment may be similar to the method for producing the underlayer light diffusion sheet 4 illustrated in
(181) Advantages
(182) The underlayer light diffusion sheet 74 of this embodiment, in which the ultrafine grooves 76 are provided on the certain region extending from one end to the other end of the back face of the protective layer 75, is capable of inhibiting the creation of hot spots. The underlayer light diffusion sheet 74, in which the region of the back face of the protective layer 75 that is not provided with the ultrafine grooves 76 is a flat surface, is capable of inhibiting an increase in the amount of rays of light transmitted in the width direction of the ultrafine grooves 76, in the region other than the hot spots. The underlayer light diffusion sheet 74 is likely to allow emission of rays of light diffused substantially uniformly over the entire face thereof.
(183) Other Embodiments
(184) It is to be noted that the optical sheet for a backlight unit and the backlight unit according to the embodiments of the present invention may be employed in various modified or improved modes other than those described above. For example, in place of the light guide film mentioned above, a light guide plate may be included in the backlight unit of each of the embodiments. It is not always required that the optical sheet for a backlight unit is the underlayer light diffusion sheet of each of the embodiments. The optical sheet may be, for example, the light guide film, the prism sheet, the upper-layer light diffusion sheet or the reflection sheet illustrated in
(185) It is preferred that optical sheet for a backlight unit of each of the embodiments is disposed on the back face of a sheet body including two prism sheets bonded to each other. The sheet body including two prism sheets bonded to each other is inferior in masking properties due to an air layer being less likely to be formed between the prism sheets. Meanwhile, in the case where the optical sheet for a backlight unit of the embodiment is disposed on the back face of the sheet body, the optical sheet is capable of diffusing a greater amount of rays of light in the width direction of the ultrafine grooves, whereby the backlight unit is enabled to provide a sufficient improvement of masking properties.
(186) In the case where the optical sheet for a backlight unit of the embodiment is a light diffusion sheet (the underlayer light diffusion sheet or the upper-layer light diffusion sheet), the ultrafine grooves may be provided on the back face of the light diffusion layer and/or on the front face of the protective layer. Alternatively, the ultrafine grooves may be provided on freely-selected front faces and/or back faces of the resin layers.
(187) A freely-selected resin layer of the optical sheet for a backlight unit of the embodiment may have a certain region provided with the ultrafine grooves. For example, in the case where the optical sheet for a backlight unit of the embodiment is a light diffusion sheet, at least any one of the front face and/or the back face of the base film, the front face and/or the back face of the light diffusion layer, and/or the front face and/or the back face of the protective layer may have such a region provided with the ultrafine grooves. Any two of the base film, the light diffusion layer and the protective layer may have such a region provided with the ultrafine grooves, or the base film, the light diffusion layer and the protective layer may each have such a region provided with the ultrafine grooves.
(188) The ultrafine grooves may be provided as illustrated in, for example,
(189) The configuration of the light diffusion sheet is not limited to the aforementioned three-layer structure including the base film, the light diffusion layer and the protective layer. For example, another layer may be disposed between the base film and the light diffusion layer, and/or between the base film and the protective layer.
(190) In place of the protective layer, a sticking preventive layer in which beads are dispersed in a resin matrix may be included in the light diffusion sheet. Ultrafine grooves may be provided on the sticking preventive layer. It is not always required that the light diffusion layer includes the protective layer.
(191) The light diffusion layer of the light diffusion sheet does not need to contain beads and a binder for the beads. Alternatively, the front face of the resin layer may be embossed. In addition, ultrafine grooves may be provided on the face provided with ultrafine projections and recesses formed by embossing.
(192) The optical sheet for a backlight unit of each of the embodiments may include a functional layer having on the front face thereof projections and recesses. In the case where such a functional layer is included in the optical sheet for a backlight unit of the embodiment, the functional layer may be a resin layer, and ultrafine grooves may be provided on the front face or the back face of the functional layer. Ultrafine grooves may be provided on the front face or the back face of another layer laminated on the functional layer. The projections and recesses may be shaped into embossments, prisms, waves, or the like.
(193) The specific shape of the ultrafine grooves is not limited to the shapes mentioned in the embodiments describe above, and may be, for example, a shape having a squared U-shape cross section as illustrated in
(194) Although the backlight unit of the embodiment preferably includes a plurality of LED light sources, the backlight may include only one LED light source. The specific kind of the optical sheet of the backlight unit is not particularly limited. Although the backlight unit preferably includes a plurality optical sheets on the front face side of the light guide film, the backlight unit may include only one optical sheet.
(195) The backlight unit of the embodiment is not necessarily an edge-lit backlight unit, and may be, for example, a direct-lit backlight unit.
(196) The backlight unit of the embodiment may be included in a comparatively large-sized visual display unit such as a personal computer or a liquid crystal television, or may be included in a mobile phone terminal such as a smartphone or a personal digital assistance such as a tablet terminal.
EXAMPLES
(197) Hereinafter, the embodiments of the present invention will be described in more detail by way of Examples; however, the present invention is not in any way limited to these Examples.
(198) No. 1
(199) A resin that was for forming a base film and contained polyethylene terephthalate as a principal component was subjected to extrusion molding using a T die, and then the shape of ultrafine grooves was transferred to one face of the extrusion-molded article by using a mold having on the surface thereof a reversal shape of the ultrafine grooves, whereby a base film having an average thickness of 75 m was produced. Then, a light diffusion layer containing beads and a binder was laminated on the face of the base film provided with the ultrafine grooves, whereby the light diffusion sheet of No. 1 was obtained. In the light diffusion sheet, the difference between the refractive index of the base film and the refractive index of the binder was 0.09. As to the light diffusion sheet, the average width of the ultrafine grooves was 9.3 m, the average depth thereof was 2.8 m, the average pitch thereof was 9.3 m, the standard deviation of the pitches of the ultrafine grooves was 6.54 m, the standard deviation of the depths of the ultrafine grooves was 1.13 m, and the arithmetic average roughness (Ra) in the direction perpendicular to the orientation of the ultrafine grooves was 1.34 m.
(200) No. 2
(201) A sheet body having an average thickness of 75 m was formed by using a resin similar to the resin used in No. 1. Then, ultrafine grooves were formed on one face of the sheet body by laser processing, whereby a base film was produced. Subsequently, a light diffusion layer containing beads and a binder similar to those used in No. 1 was laminated on the face of the base film provided with the ultrafine grooves, whereby the light diffusion sheet of No. 2 was obtained. As to the light diffusion sheet, the average width of the ultrafine grooves was 26.9 m, the average depth thereof was 6.44 m, the average pitch thereof was 26.9 m, the standard deviation of the pitches of the ultrafine grooves was 5.56 m, the standard deviation of the depths of the ultrafine grooves was 2.38 m, and the arithmetic average roughness (Ra) in the direction perpendicular to the orientation of the ultrafine grooves was 0.92 m.
(202) No. 3
(203) A sheet body having an average thickness of 75 m was formed by using a resin similar to the resin used in No. 1. Then, ultrafine grooves were formed on one face of the sheet body by filing, whereby a base film was produced. Subsequently, a light diffusion layer containing beads and a binder similar to those used in No. 1 was laminated on the face of the base film provided with the ultrafine grooves, whereby the light diffusion sheet of No. 3 was obtained. As to the light diffusion sheet, the average width of the ultrafine grooves was 1.0 m, the average length thereof was 30 mm, the average depth thereof was 0.5 m, the average pitch thereof was 18.84 m, the standard deviation of the pitches of the ultrafine grooves was 8.29 m, the standard deviation of the depths of the ultrafine grooves was 0.56 m, and the arithmetic average roughness (Ra) in the direction perpendicular to the orientation of the ultrafine grooves was 0.30 m.
(204) No. 4
(205) A sheet body having an average thickness of 75 m was formed by using a resin similar to the resin used in No. 1. Then, ultrafine grooves were formed on one face of the sheet body by using a cutting tool, whereby a base film was produced. Subsequently, a light diffusion layer containing beads and a binder similar to those used in No. 1 was laminated on the face of the base film provided with the ultrafine grooves, whereby the light diffusion sheet of No. 4 was obtained. As to the light diffusion sheet, the average width of the ultrafine grooves was 32.7 m, the average depth thereof was 28.1 m, the average pitch thereof was 31.5 m, the standard deviation of the pitches of the ultrafine grooves was 9.73 m, the standard deviation of the depths of the ultrafine grooves was 0.89 m, and the arithmetic average roughness (Ra) in the direction perpendicular to the orientation of the ultrafine grooves was 4.30 m.
(206) No. 5
(207) The light diffusion sheet of No. 5 was obtained as in No. 1, except that the ultrafine grooves were not formed.
(208) The properties of the light diffusion sheets of No. 1 to No. 5 are shown in Table 1.
(209) TABLE-US-00001 TABLE 1 Arithmetic Average Roughness Difference in (Ra) in Refractive Ultrafine Grooves Direction Average Index Standard Standard Perpendicular Thickness between Average Average Average Average Deviation Deviation to Orientation of Base Base Film Width Length Depth Pitch of Pitches of Depths of Ultrafine Film (m) and Binder (m) (mm) (m) (m) (m) (m) Grooves (m) No. 1 75 0.09 9.3 2.8 9.3 6.54 1.13 1.34 No. 2 75 0.09 26.9 6.44 26.9 5.56 2.38 0.92 No. 3 75 0.09 1.0 30 0.5 18.84 8.29 0.56 0.30 No. 4 75 0.09 32.7 28.1 31.5 9.73 0.89 4.30 No. 5 75 0.09
Examples 1 to 5
(210) The light diffusion sheet of No. 1 was laminated on a front face side of a light guide film of an edge-lit backlight unit that included LED light sources and was to be included in a liquid crystal display device in such a manner that the average orientation of the ultrafine grooves with respect to the average direction of the rays of light emitted by the LED light sources and incident on the light guide film was directed at an angle shown in Table 2.
Examples 6 to 10
(211) The light diffusion sheet of No. 2 was laminated on a front face side of a light guide film of an edge-lit backlight unit that included LED light sources and was to be included in a liquid crystal display device in such a manner that the average orientation of the ultrafine grooves with respect to the average direction of the rays of light emitted by the LED light sources and incident on the light guide film was directed at an angle shown in Table 2.
Examples 11 to 15
(212) The light diffusion sheet of No. 3 was laminated on a front face side of a light guide film of an edge-lit backlight unit that included LED light sources and was to be included in a liquid crystal display device in such a manner that the average orientation of the ultrafine grooves with respect to the average direction of the rays of light emitted by the LED light sources and incident on the light guide film was directed at an angle shown in Table 2.
Examples 16 to 20
(213) The light diffusion sheet of No. 4 was laminated on a front face side of a light guide film of an edge-lit backlight unit that included LED light sources and was to be included in a liquid crystal display device in such a manner that the average orientation of the ultrafine grooves with respect to the average direction of the rays of light emitted by the LED light sources and incident on the light guide film was directed at an angle shown in Table 2.
Comparative Example
(214) The light diffusion sheet of No. 5 was laminated on a front face side of a light guide film of an edge-lit backlight unit that included LED light sources and was to be included in a liquid crystal display device.
(215) Half-Value Angle
(216) For each of Examples 1 to 20 and Comparative Example, a half-value angle associated with the face luminance of the light diffusion sheet was measured by using EzContrast available from ELDIM. The results of the measurement are shown in Table 2.
(217) Lack in Uniformity of Luminance
(218) The backlight unit of each of Examples 1 to 20 and Comparative Example was installed in the liquid crystal display device, and then the image displayed on the liquid crystal display device was observed. The presence or absence of the lack in uniformity of luminance was determined by a visual observation, and evaluations were made in accordance with the following criteria.
(219) A: The lack in uniformity of luminance was not visible at all.
(220) B: When the image was observed carefully, the lack in uniformity was slightly visible in the vicinity of the light sources in a planar view.
(221) C: Even when the image was observed less carefully, the lack in uniformity of luminance was slightly visible in the vicinity of the light sources in a planar view.
(222) D: Even when the image was observed less carefully, the lack in uniformity of luminance was visible.
(223) TABLE-US-00002 TABLE 2 Average Orientation of Ultrafine Grooves with Respect Half-Value Angle () to Average Direction Direction of Parallel Direction Rays of Light to Rays Perpendicular Lack in Emitted by of Light to Uniformity LED Light White Rays of Light of Sources Light White Light Luminance Example 1 0 10 50 A Example 2 15 10 50 A Example 3 20 15 45 A Example 4 30 25 35 B Example 5 45 29 31 C Example 6 0 10 50 A Example 7 15 10 50 A Example 8 20 12 47 A Example 9 30 28 35 B Example 10 45 29 31 C Example 11 0 20 40 A Example 12 15 22 36 A Example 13 20 25 35 B Example 14 30 28 32 B Example 15 45 29 31 C Example 16 0 8 52 A Example 17 15 8 52 A Example 18 20 12 47 A Example 19 30 27 33 B Example 20 45 29 31 C Comparative 30 30 D Example
Evaluation Results
(224) As shown in Table 2, it was revealed that the half-value angle associated with the luminance in the direction perpendicular to the rays of light emitted by the LED light sources in each of Examples 1 to 20, in which the average orientation of the ultrafine grooves with respect to the average direction of the rays of light emitted by the LED light sources and incident on the light guide film was directed at an angle of 45 or less, was greater than the half-value angle measured in Comparative Example, and thus the lack in uniformity of luminance was likely to be inhibited. It was also revealed that the half-value angle associated with the luminance in the direction perpendicular to the rays of light emitted by the LED light sources increased as the average angle at which the ultrafine grooves were oriented decreased, and thus the lack in uniformity of luminance was likely to be inhibited. Furthermore, it was revealed that Examples 1 to 5 in which the ultrafine grooves were formed by using the mold, Examples 6 to 10 in which the ultrafine grooves were formed by laser processing, Examples 16 to 20 in which the ultrafine grooves were formed by using a cutting tool, enabled formation of more desirable ultrafine grooves as compared to Examples 11 to 15 in which the ultrafine grooves were formed by filing, and that the more desirable fine grooves yielded a greater half-value angle associated with the luminance in the direction perpendicular to the rays of light emitted by the LED light sources, and the lack in uniformity of luminance was likely to be inhibited accordingly. In addition, as shown in
INDUSTRIAL APPLICABILITY
(225) As described in the foregoing, the optical sheet for a backlight unit and the backlight unit according to the embodiments of the present invention are capable of inhibiting the creation of hot spots, and are thus suited for use in various types of liquid crystal display devices such as high-quality transmissive liquid crystal display devices.
EXPLANATION OF THE REFERENCE SYMBOLS
(226) 1 light guide film
(227) 2, 82 LED light source
(228) 3 optical sheet
(229) 4, 24, 34, 44, 54, 64, 74 underlayer light diffusion sheet
(230) 5 first prism sheet
(231) 6 second prism sheet
(232) 7 upper-layer light diffusion sheet
(233) 8 reflection sheet
(234) 11, 25, 35 base film
(235) 12, 36, 45 light diffusion layer
(236) 13, 26, 37, 75 protective layer
(237) 14, 38, 46 bead
(238) 15, 39, 47 binder
(239) 16, 27, 40, 48, 76, 86 ultrafine groove
(240) 17 recessed portion
(241) 18 raised portion
(242) 101 edge-lit backlight unit
(243) 102 light source
(244) 103 light-guiding sheet
(245) 104 optical sheet
(246) 105 reflection sheet
(247) 106 underlayer light diffusion sheet
(248) 107 prism sheet
(249) 108 upper-layer light diffusion sheet