Extruded molds and methods for manufacturing composite truck panels
10538051 ยท 2020-01-21
Assignee
Inventors
Cpc classification
B29K2105/0854
PERFORMING OPERATIONS; TRANSPORTING
B32B2250/44
PERFORMING OPERATIONS; TRANSPORTING
B29C39/003
PERFORMING OPERATIONS; TRANSPORTING
B32B27/12
PERFORMING OPERATIONS; TRANSPORTING
B32B2250/244
PERFORMING OPERATIONS; TRANSPORTING
B29K2067/00
PERFORMING OPERATIONS; TRANSPORTING
B32B2307/714
PERFORMING OPERATIONS; TRANSPORTING
B29C70/48
PERFORMING OPERATIONS; TRANSPORTING
B29C33/3842
PERFORMING OPERATIONS; TRANSPORTING
B32B5/18
PERFORMING OPERATIONS; TRANSPORTING
B32B2307/718
PERFORMING OPERATIONS; TRANSPORTING
B29C33/42
PERFORMING OPERATIONS; TRANSPORTING
B29L2031/3002
PERFORMING OPERATIONS; TRANSPORTING
B29C39/10
PERFORMING OPERATIONS; TRANSPORTING
B29K2075/00
PERFORMING OPERATIONS; TRANSPORTING
B29C37/0032
PERFORMING OPERATIONS; TRANSPORTING
B32B2260/021
PERFORMING OPERATIONS; TRANSPORTING
B29C39/026
PERFORMING OPERATIONS; TRANSPORTING
B32B2250/40
PERFORMING OPERATIONS; TRANSPORTING
B32B3/30
PERFORMING OPERATIONS; TRANSPORTING
B29C2037/0035
PERFORMING OPERATIONS; TRANSPORTING
International classification
B29C70/02
PERFORMING OPERATIONS; TRANSPORTING
B32B27/12
PERFORMING OPERATIONS; TRANSPORTING
B32B3/30
PERFORMING OPERATIONS; TRANSPORTING
B29C39/00
PERFORMING OPERATIONS; TRANSPORTING
B29C39/10
PERFORMING OPERATIONS; TRANSPORTING
B32B5/02
PERFORMING OPERATIONS; TRANSPORTING
B32B5/18
PERFORMING OPERATIONS; TRANSPORTING
B29C33/38
PERFORMING OPERATIONS; TRANSPORTING
B29C70/48
PERFORMING OPERATIONS; TRANSPORTING
Abstract
Extruded molds and methods for manufacturing composite structures using the extruded molds are disclosed. The molds may include recessed or raised longitudinal features to impart a corresponding shape to the molded composite structures. The composite structures may be panels used to construct cargo vehicles, for example.
Claims
1. A method of manufacturing a composite structure comprising: providing a mold body having a mold surface with: a first portion that is flat; a second portion that is flat; and a third portion that deviates from being flat; forming a fiber-reinforced plastic composite structure upon the mold surface, a molded surface of the composite structure having: a first portion corresponding to the first portion of the mold surface; a second portion corresponding to the second portion of the mold surface; and a third portion corresponding to the third portion of the mold surface, wherein the third portion extends across an entire length of the composite structure; and directing a heat exchange fluid through a substantially hollow interior of the mold body, wherein the mold body includes a plurality of individually extruded segments that are coupled together and cooperate to define the mold surface.
2. The method of claim 1, wherein each segment extends an entire length of the mold body and a partial width of the mold body.
3. The method of claim 1, wherein each segment has a width of about 0.5-2 feet.
4. The method of claim 1, wherein the plurality of segments are identical to each other.
5. A method of manufacturing a composite structure comprising: providing an extruded mold body having a mold surface by coupling together a plurality of individually extruded segments that cooperate to define the mold surface; forming the composite structure upon the mold surface, the composite structure comprising: a first end; a second end; and a molded surface including: a first portion that is flat; a second portion that is flat; and a third portion that deviates from being flat, wherein the third portion extends entirely from the first end to the second end; and directing a heat exchange fluid through a substantially hollow interior of the mold body.
6. The method of claim 5, wherein the composite is a fiber-reinforced plastic.
7. The method of claim 5, wherein the mold body is extruded along a longitudinal axis, and the third portion extends parallel to the longitudinal axis.
8. The method of claim 5, wherein the third portion is a channel that is recessed between the first and second portions.
9. The method of claim 5, wherein the composite panel is one of a floor, a roof, a sidewall, and a nose for a cargo vehicle.
10. A method of manufacturing a composite structure comprising: providing an extruded mold body having a mold surface by coupling together a plurality of individually extruded segments that cooperate to define the mold surface; forming the composite structure upon the mold surface, wherein the mold surface includes: a first portion that is flat; a second portion that is flat; and a third portion that deviates from being flat, wherein the third portion extends parallel to a longitudinal axis of the extruded mold body; and directing a heat exchange fluid through a substantially hollow interior of the mold body.
11. The method of claim 10, wherein the third portion is a channel that is recessed between the first and second portions.
12. The method of claim 10, wherein the third portion extends entirely from a first end to a second end of the mold body.
13. The method of claim 10, wherein the extruded mold body interacts with a second mold body to form the composite structure therebetween.
14. The method of claim 10, wherein the forming step comprises: applying a resin layer onto the mold surface; inserting reinforcing materials into the resin layer; and allowing the reinforced resin layer to cure.
15. The method of claim 10, wherein: the providing step comprises providing the mold body having a width of about 8-12 feet and a length of about 20-50 feet; and the forming step comprises forming the composite structure having a width of about 8-12 feet and a length of about 20-50 feet.
16. The method of claim 10, wherein each segment extends an entire length of the mold body such that the coupling step comprises arranging the plurality of extruded segments across a width of the mold body.
17. The method of claim 10, wherein the mold body is metallic.
18. The method of claim 17, wherein the mold body is constructed of aluminum.
19. The method of claim 10, wherein the composite structure is a fiber-reinforced plastic.
20. A method of manufacturing a composite structure comprising: providing an extruded mold body having a mold surface by coupling together a plurality of individually extruded segments that cooperate to define the mold surface, wherein the providing step comprises providing the mold surface having: a first portion that is flat; a second portion that is flat; and a third portion that deviates from being flat; and forming the composite structure upon the mold surface, wherein the forming step comprises forming a molded surface of the composite structure having: a first portion corresponding to the first portion of the mold surface; a second portion corresponding to the second portion of the mold surface; and a third portion corresponding to the third portion of the mold surface, wherein the third portion extends across an entire length of the composite structure; and directing a heat exchange fluid through a substantially hollow interior of the mold body.
21. The method of claim 20, wherein: the third portion of the mold surface is a longitudinal ridge between the first and second portions; and the third portion of the molded surface is a longitudinal channel.
22. A method of manufacturing a composite structure comprising: providing a mold body formed by extrusion and having a mold surface with: a first portion that is flat; a second portion that is flat; and a third portion that deviates from being flat; forming a fiber-reinforced plastic composite structure upon the mold surface, a molded surface of the composite structure having: a first portion corresponding to the first portion of the mold surface; a second portion corresponding to the second portion of the mold surface; and a third portion corresponding to the third portion of the mold surface, wherein the third portion extends across an entire length of the composite structure; and directing a heat exchange fluid through a substantially hollow interior of the mold body.
23. The method of claim 22, wherein the mold body has a width of about 8-12 feet and a length of about 20-50 feet.
24. The method of claim 22, wherein the third portion of the mold body is formed by extrusion and extends across an entire length of the mold body.
25. The method of claim 22, wherein the mold body is metallic.
26. The method of claim 22, wherein: the third portion of the mold surface is a longitudinal ridge between the first and second portions; and the third portion of the molded surface is a longitudinal channel.
27. The method of claim 22, wherein the forming step comprises applying a gel coat polyester resin onto the mold surface to form the molded surface of the composite structure.
28. The method of claim 26, wherein the forming step further comprises applying an extruded preform assembly of a non-woven spun bond polymeric material and a polymeric foam core onto the gel coat polyester resin.
29. The method of claim 22, wherein the molded surface includes a plurality of features similar to the third portion, the plurality of features being spaced apart and separated by flat portions similar to the first and second portions.
30. The method of claim 22, further comprising: removing the composite structure from the mold body; rotating the composite structure 180 degrees such that the molded surface faces upward; and installing the composite structure as a floor in a cargo vehicle.
Description
BRIEF DESCRIPTION OF THE DRAWINGS
(1) The foregoing aspects and many of the intended advantages of this invention will become more readily appreciated as the same becomes better understood by reference to the following detailed description when taken in conjunction with the accompanying drawings.
(2)
(3)
(4)
(5)
(6)
(7)
(8)
(9) Corresponding reference characters indicate corresponding parts throughout the several views. Although the drawings represent embodiments of various features and components according to the present disclosure, the drawings are not necessarily to scale and certain features may be exaggerated in order to better illustrate and explain the present disclosure. The exemplification set out herein illustrates an embodiment of the invention, and such an exemplification is not to be construed as limiting the scope of the invention in any manner.
DETAILED DESCRIPTION OF THE DRAWINGS
(10) For the purposes of promoting an understanding of the principals of the invention, reference will now be made to the embodiments illustrated in the drawings, which are described below. The embodiments disclosed below are not intended to be exhaustive or limit the invention to the precise form disclosed in the following detailed description. Rather, the embodiments are chosen and described so that others skilled in the art may utilize their teachings. It will be understood that no limitation of the scope of the invention is thereby intended. The invention includes any alterations and further modifications in the illustrative devices and described methods and further applications of the principles of the invention which would normally occur to one skilled in the art to which the invention relates.
(11) 1. Cargo Vehicle
(12) Referring initially to
(13) In the illustrated embodiment of
(14) 2. Composite Panels
(15) Various panels of the cargo body 120 may be constructed, at least in part, of composite materials. For example, the floor 130, roof 140, right and left sidewalls 150, and/or nose 160 of the cargo body 120 may be constructed of composite materials. As such, the floor 130, roof 140, right and left sidewalls 150, and/or nose 160 of the cargo body 120, may be referred to herein as composite panels.
(16) Composite structures are generally formed by combining two or more different constituents that remain separate and distinct in the final composite material. Exemplary composite materials include fiber-reinforced plastics (FRP), for example carbon-fiber reinforced plastics (CRP). These composite structures may lack internal metal components. Also, each composite panel may be a single, unitary component, which may be formed from a plurality of layers permanently coupled together, as discussed further below.
(17) The composite construction of the cargo body 120 may present certain advantages. For example, the composite cargo body 120 may be lighter in weight than a typical metallic cargo body, which may improve fuel efficiency. Also, the composite cargo body 120 may have fewer metallic structures than a typical cargo body, which may make the cargo body 120 less susceptible to corrosion and heat loss. Additionally, the composite cargo body 120 may include fewer parts than a typical metallic cargo body, which may simplify construction, reduce inventory, and reduce variation in manufacturing. Further, the composite cargo body 120 may be suitable for use with sensitive cargo, including foodstuffs, because the composite materials may be inert to avoid reacting with the cargo and other materials and because the composite materials may be easy to clean and maintain to ensure proper hygiene. As a result, the composite cargo body 120 may qualify as food grade equipment.
(18) Referring next to
(19) The illustrative composite floor 130 is generally rectangular in shape and extends along the longitudinal axis L of the vehicle 100 (
(20) The composite floor 130 also includes an upper floor surface 134 and a lower floor surface 135. The upper floor surface 134 includes flat portions 136 for supporting cargo. The upper floor surface 134 may also include various longitudinal features that deviate from the flat portions 136 and extend parallel to the longitudinal axis L. For example, as shown in
(21) The size and shape of the composite floor 130 may vary to accommodate different vehicles 100. In the illustrated embodiment of
(22) Additional information regarding composite structures is disclosed in the following patents and published patent applications, each of which is incorporated by reference in its entirety herein: U.S. Pat. Nos. 5,429,066, 5,800,749, 5,664,518, 5,897,818, 6,013,213, 6,004,492, 5,908,591, 6,497,190, 6,911,252, 5,830,308, 6,755,998, 6,496,190, 6,911,252, 6,723,273, 6,869,561, 8,474,871, 6,206,669, and 6,543,469, and U.S. Patent Application Publication Nos. 2014/0262011 and 2014/0199551. Exemplary composite structures include DuraPlate structures provided by Wabash National Corporation of Lafayette, Ind. and PRISMA structures provided by Compsys, Inc. of Melbourne, Fla.
(23) 3. Mold
(24) Referring next to
(25) The illustrative mold assembly 300 includes a mold body 310, a base 330, and a frame 340 having castor wheels 342 to facilitate movement of the mold assembly 300. The mold assembly 300 may also include brackets (not shown) to facilitate lifting and transporting the mold assembly 300, such as using a crane.
(26) As shown by comparing
(27) The mold body 310 also includes an upper mold surface 314 and a lower mold surface 315. The upper mold surface 314 is a negative mold for the resulting upper floor surface 134, such that the upper floor surface 134 can be formed upon the upper mold surface 314, as discussed further below. The upper mold surface 314 includes flat portions 316. Any unintended gaps or defects in the upper mold surface 314 may be filled with a suitable filler 317 (e.g., metal rods, wax) to provide this flat surface. The upper mold surface 314 may also include various longitudinal features that deviate from the flat portions 316 and extend parallel to the longitudinal axis L to form the opposite longitudinal features in the upper floor surface 134. For example, as shown by comparing
(28) Between the upper mold surface 314 and the lower mold surface 315, the mold body 310 may be substantially hollow except for a plurality of spaced-apart internal supports 319. The hollow construction of the mold body 310 may accommodate a heat exchange fluid (e.g., air, water) inside the mold body 310 to control the temperature of the upper mold surface 314 during molding, as discussed further below.
(29) According to an exemplary embodiment of the present disclosure, the mold body 310 is formed by extrusion along the longitudinal axis L from the front end 312 to the rear end 313. More specifically, the mold body 310 may be formed by passing material through a die along the longitudinal axis L, where the die has a desired cross-section in a direction perpendicular to the longitudinal axis L. As such, the mold body 310 may be referred to herein as an extruded mold body 310. Because the features in the upper mold surface 314 of the mold body 310 (e.g., the flat portions 316, the ridges 318) are also formed by extrusion, these features may extend along the longitudinal axis L entirely from the front end 312 to the rear end 313. The mold body 310 may be constructed of metal (e.g., aluminum) or another material that is suitable for extrusion.
(30) To accommodate standard extrusion equipment, the mold body 310 may be divided into a plurality of individually extruded segments 320 across the width w.sub.m. The illustrative mold body 310 includes nine segments 320, with each segment 320 accounting for 1/9 of the width w.sub.m, but this number may vary. The width w.sub.s of each segment 320 may be about 0.5-2 feet, and the length l.sub.s of each segment may be the same as the overall length l.sub.m of the mold body 310 itself. For simplicity of construction, the segments 320 may be identical to one another and trimmed to the desired length.
(31)
(32) The extruded construction of the mold body 310 may present certain advantages. First, the extruded mold body 310 may be less expensive than a machined mold body. Second, the extruded mold body 310 may be more durable than a cast (e.g., fiberglass) mold body. Third, the extruded mold body 310 may be repaired, if necessary, such as by removing and replacing a damaged segment 320 while retaining the other segments 320. Finally, the profile of the upper mold surface 314 may be customized to create desired features in the upper floor surface 130 (
(33) 4. Molding Process
(34) Referring next to
(35) In step 702, the upper mold surface 314 of the mold body 310 may be prepared for molding. For example, the upper mold surface 314 may be cleaned and/or pretreated with a release agent (e.g., wax) to facilitate separation after molding.
(36) In step 704, a first resin layer 600 is applied onto the upper mold surface 314 of the mold body 310. An exemplary first resin is a gel coat polyester resin. The first resin layer 600 may be applied across the mold body 310 in liquid form by spraying, rolling, brushing, or calendaring, for example. The first resin layer coats the negative space above the upper mold surface 314.
(37) In step 706, the first resin layer 600 is allowed to cure using a suitable curing catalyst. Ultimately, the first resin layer 600 will take on the opposite profile of the upper mold surface 314 to form the upper floor surface 134 of the composite floor 130.
(38) In step 708, one or more reinforcing materials 604 are applied onto the cured first resin layer 600 from step 706. Exemplary reinforcing materials 604 include woven or stitched fiberglass cloth sheets, for example. Other exemplary reinforcing materials 604 include extruded preform assemblies of a woven or stitched fiberglass cloth, a non-woven spun bond polymeric (e.g., polyester) material, and a polymeric (e.g., polyurethane) foam core, for example. The spun bond polymeric material may be mechanically stitched to the fiberglass cloth and/or the foam. In one embodiment, the spun bond material may be a polyester material, the foam may be a polyurethane material, and the resin may be a thermoset plastic resin matrix. Such preforms and any other reinforcing materials 604 may be shaped, cut to size, and arranged on the mold assembly 300 in a manner that accommodates the strength requirements of the final structure. In areas of the final structure requiring less strength, the preforms may be relatively large in size, with the foam cores spanning relatively large distances before reaching the surrounding fiberglass and polymeric skins. By contrast, in areas of the final structure requiring more strength, the preforms may be relatively small in size, with the foam cores spanning relatively small distances before reaching the surrounding fiberglass and polymeric skins. For example, the preforms may be shaped as relatively wide panels in areas of the final structure requiring less strength and as relatively narrow support beams in areas of the final structure requiring more strength. Other exemplary techniques for strengthening such support beams include reinforcing the outer skins, such as by using uni-directional glass fibers or additional cloth in the outer skins, and/or reinforcing the inner cores, such as by using hard plastic blocks or higher density foam in the inner cores.
(39) In step 710, a second liquid resin layer 602 is applied and worked into the reinforcing materials 604 to wet the reinforcing materials 604 with the second resin 602. An exemplary second resin is a polyester resin, which may be similar to the first resin. An exemplary resin is the co-cure resin disclosed in U.S. Pat. No. 9,371,468, which is incorporated by reference in its entirety herein.
(40) In step 712, the reinforced second resin layer 602 is allowed to cure using a suitable curing catalyst. During curing, the reinforcing materials 604 may be forced into close contact with the second liquid resin layer 602 by applying pressure on top of the reinforcing materials 604 and/or by applying a vacuum to the reinforcing materials 604, for example. Once cured, the second resin layer 602 becomes permanently coupled to the reinforcing materials 604 and the first resin layer 600 to form a single structure. Steps 708-712 may be repeated one or more times. In certain embodiments, the first curing step 706 may be performed together with the second curing step 712. In other words, the curing steps 706, 712 may be performed simultaneously.
(41) In step 714, a third resin layer 606 may be applied onto the cured second resin layer 602. An exemplary third resin is a polyester resin, which may be similar to the first and/or second resins.
(42) In step 716, the third resin layer 606 is allowed to cure using a suitable curing catalyst. Once cured, the third resin layer becomes permanently coupled to the first resin layer 600 and second resin layer 602 to form a single structure. Ultimately, the third resin layer 606 may form the lower floor surface 135 of the composite floor 130. It is also within the scope of the present disclosure for the third resin layer 606 to be eliminated and for the reinforced second resin layer 602 to form the lower floor surface 135 of the composite floor 130. In certain embodiments, the first curing step 706 and the second curing step 712 may be performed together with the third curing step 716. In other words, the curing steps 706, 712, 716 may be performed simultaneously.
(43) In step 718, the composite floor 130 is removed from the mold body 310 and flipped over 180 degrees such that the upper floor surface 134 that was facing downward toward the mold body 310 now faces upward. If necessary, the outer perimeter of the composite floor 130 may be trimmed to desired dimensions for use in vehicle 100 (
(44) As indicated above, a heat exchange fluid (e.g., air, water) may be introduced (e.g., pumped) into the hollow mold body 310 to control the temperature of the upper mold surface 314 during the molding process 700. For example, to slow down or otherwise control a curing step 706, 712, 716, a cold heat exchange fluid may be introduced into the hollow mold body 310. Using a cold heat exchange fluid may be particularly beneficial when the curing step 706, 712, 716, is exothermic, because the cold heat exchange fluid may remove excess heat and maintain a controlled curing temperature. To speed up or otherwise control a curing step 706, 712, 716, a hot heat exchange fluid may be introduced into the hollow mold body 310. The temperature of the mold body 310 may also be controlled by placing the mold body 310 inside a temperature-controlled environment, such as a large refrigerator, oven, or autoclave, for example. The heat exchange fluid may be circulated repeatedly through the mold body 310 as part of a heat exchange loop.
(45) Although the illustrative mold assembly 300 of
(46) The closed-molding method may be similar to the open-molding method of
(47) While this invention has been described as having an exemplary design, the present invention may be further modified within the spirit and scope of this disclosure. This application is therefore intended to cover any variations, uses, or adaptations of the invention using its general principles. Further, this application is intended to cover such departures from the present disclosure as come within known or customary practices in the art to which this invention pertains.